Look what happened to the gel coat :(


Author
Message
Jess8bit
Jess8bit
Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)
Group: Forum Members
Posts: 133, Visits: 566
http://img442.imageshack.us/img442/6315/vgyz.jpg

Apparently this occured during the shipping but the package was ok and I suspect others reasons :

- Could it be due to the fact I left the gel coat (EC GC50) cure too long (more than 24hrs), causing delamination ?

- Or would it be because of the GC50 thickness (but does not seem too thick for me) ?

any other clue ?

feel bad right now Unsure 
frustrated cause the part was ok when I sent it.
Reply
Jess8bit
Jess8bit
Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)
Group: Forum Members
Posts: 133, Visits: 566
Thank you for the trick Smile

I really need to add some woven glass to my shopping list !
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Jess8bit - 12 Years Ago
wozza - 12 Years Ago
Jess8bit - 12 Years Ago
Warren (Staff) - 12 Years Ago
Jess8bit - 12 Years Ago
Jess8bit - 12 Years Ago
carboncactus - 12 Years Ago
wozza - 12 Years Ago
Jess8bit - 12 Years Ago
wozza - 12 Years Ago
Jess8bit - 12 Years Ago
wozza - 12 Years Ago
Jess8bit - 12 Years Ago
wozza - 12 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search