Trouble with perfect finish


Author
Message
Davidpetty1988
Davidpetty1988
Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)
Group: Forum Members
Posts: 26, Visits: 89
Hi I'm doing resin infusion and I'm very happy with the glossy finish apart from some tiny gaps around the fibres on the surface finish.any ideas where I might be going wrong?
http://www.talkcomposites.com/Uploads/Images/67f73a13-efe7-4660-8fd7-f42f.jpg
I hope its a clear enough picture thanks in advance 
Dave
VVS
VVS
Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)
Group: Moderators
Posts: 226, Visits: 334
hi, looks dry
try leaving the resin side clamp off for longer.
Davidpetty1988
Davidpetty1988
Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)
Group: Forum Members
Posts: 26, Visits: 89
So clamp the vac side first then leave the resin side pumping for another 20-30 secs then clamp the resin side off is this what you mean I read something like this in another post didn't no weather it was applicable to my problem.It quite confusing in the ec guide it tells you to do it another conflicting info.
Its a pretty glossy finish to be dry isn't it?
http://www.talkcomposites.com/Uploads/Images/c952cfa6-c3a0-44fc-b1d2-1467.jpg
Edited 10 Years Ago by Davidpetty1988
Hanaldo
Hanaldo
Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
It's dry. You have either clamped the resin too early, or you have allowed too much resin to be drawn out of the laminate after clamping the resin line. 

Don't clamp the resin feed first. Either clamp at the same time, or if a cosmetic finish is paramount, clamp the vacuum line first and then after 20-30 seconds clamp the resin line. 
Edited 10 Years Ago by Hanaldo
Davidpetty1988
Davidpetty1988
Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)Supreme Being (442 reputation)
Group: Forum Members
Posts: 26, Visits: 89
Thanks very much guys will do that on my next peice . 
Dammit I love this forum site all you guys are awsome !!!!
Dave
davro
davro
Supreme Being (4.1K reputation)Supreme Being (4.1K reputation)Supreme Being (4.1K reputation)Supreme Being (4.1K reputation)Supreme Being (4.1K reputation)Supreme Being (4.1K reputation)Supreme Being (4.1K reputation)Supreme Being (4.1K reputation)Supreme Being (4.1K reputation)
Group: Forum Members
Posts: 300, Visits: 2.2K
As previously said clamp the resin output line first and allow the vacuum in the bag to suck in some resin before clamping the resin input line this should give you a nice resin rich part, without the pin holes Smile 

The clamping time can vary depending on the area of the sheet your pulling.



David Stevens
YouTubeComment | Rate | Subscribe
Instagram

Composite Projects
Body Package for Dax Rush
RC Car Touring Body 1/10 Scale


Edited 10 Years Ago by davro
GO