Help


Author
Message
111mattin111
111mattin111
Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)
Group: Forum Members
Posts: 67, Visits: 910
Ok so sorted the leak out and no pressure drop after couple of hours then the nightmare started mixed up the resin 3kg mix

Started the infuse started really well then stopped flowing as quick where the resin enters there was a big puddle of resin like it wasn't being pulled through the part for some reason

The hoses from pump to catch pot ect seemed collapsed so clamped the bag off put new lines on and it started pulling the resin through again but by this point it had started to gel so wouldn't finish infusing the part not a clue what happened as I did everything by the book

So one BIG FAIL 😢
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Just ironing out the kinks mate, happens to everyone when they first start infusing. Keep at it, you'll get it sorted. 

Sounds like you used some cheap hose that couldn't take the vacuum. You need some fairly rigid stuff, so if you can squeeze it closed with your fingers then I'd suggest finding something else. 
111mattin111
111mattin111
Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)
Group: Forum Members
Posts: 67, Visits: 910
I used the hose that comes with the infusion starter kit, which other hose would you recommend? 
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
I see. Well in that case, I'd probably get in contact with the guys at EC, as their stuff definitely shouldn't collapse under vacuum. 
111mattin111
111mattin111
Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)
Group: Forum Members
Posts: 67, Visits: 910
I thought that, I now think it was definitely down to collapsed pipes as soon as I changed them it progressed again but was to late to fully infuse as it was gelling over night it got a little further but there's still a patch it didn't get to, 
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
I have used the EC clear hose many times and the only time it has collapsed is when its been too warm IE if you have a blower heater etc directed at the hose, when your infusing large parts you can mix your resin in smaller batches and use a slow resin. You will need another pump and a degas chamber to use this method.
Regards Chris 

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
111mattin111
111mattin111
Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)
Group: Forum Members
Posts: 67, Visits: 910
I mixed the resin with slow hardner, I didn't have any blow heaters on it was done in the house, the places where it had collapsed were at the barb on the pump, where it entered the catch pot and where I'd previously had it clamped for drop test
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
OK so that's a slightly different issue and can happen with this type of hose, when you have started to infuse slacken off the clamp and turn it 90 degrees at the same point and tighten it up slightly and this will open the pipe up again. This only seems to happen when the clamp has been in place for a number of hours.
Reagrds Chris

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
Edited 10 Years Ago by carbonfibreworks
111mattin111
111mattin111
Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)Supreme Being (449 reputation)
Group: Forum Members
Posts: 67, Visits: 910
I did try that putting the clamp back on and trying to squash the pipe back the other way, I think if I'd of changed the pipes sooner it would of all gone ok, 
What would of caused the swamp of resin around the entry point there was that much resin that the bag went saggy, but once I changed the pipes it started to draw it out and tighten the bag again, 

Bags been fine over night no pressure drop just a shame the whole part didn't infuse 
Frobisher
Frobisher
Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)
Group: Forum Members
Posts: 14, Visits: 93
Was your resin feed pot positioned below the part? If it was higher the liquid resin could siphon which might explain the extra resin around the inlet. 
GO