Is Chopped Strand Mat compatible with resin infusion ?


Author
Message
Jess8bit
Jess8bit
Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)
Group: Forum Members
Posts: 133, Visits: 566
...or do we have to use woven glass instead ?

I need to make a thick part (3mm) so I plan to use 2 layers of 195g 2/2 twill CF, and then the rest with glass (or maybe Soric ? or combination of Soric + galss ?)

thank you Smile

J
Warren (Staff)
Warren (Staff)
Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
It would need to be a chopped strand mat which is powder bound.

It would be very difficult to infuse properly as the unwetted CSM is stiff so hard to get into awkward shapes.  Generally CSM is wetlay so as you put resin on it, it soaks in and the CSM goes floppy.

I would suggest you use soric.  The part will be lighter and stiffer.  If you want to add more layers than just the CF then woven glass is the way forward.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Jess8bit
Jess8bit
Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)
Group: Forum Members
Posts: 133, Visits: 566
Thank you Warren,

I only have CSM emulsion bound in stock (the one I use with Uni Mould, as EC advises to).

I have some 2mm soric so I'll give it a try with, but I understand I'll need to order woven glass if I want to make thicker parts.

Regards,
Jess.
carboncactus
carboncactus
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 243, Visits: 1K
Emulsion bound and epoxy is a deffinite no go.
I might be wrong but if you use a core material, it preferably wants to be a symetric layup, so to get it close to 3mm:

195gsm CF
195gsm CF
2mm Soric
195gsm CF
195gsm CF

If you dont do it symmetrically, one side will be stiffer than the other and cause warping. Again this is what I've heard, I might be wrong.

You could use your CSM, but you would have to use a polyester infusion resin, like the one from east coast, or a vinylester, tight corners might be an issue, but it depends, a bonnet might be fine. If you use a polyester, you'd kill 2 birds with one stone and have UV protection.

http://www.talkcomposites.com/Uploads/Images/db628ad5-e0e7-47b9-873a-3d84.png
Edited 13 Years Ago by carboncactus
Jess8bit
Jess8bit
Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)
Group: Forum Members
Posts: 133, Visits: 566
Great advice Carbon Cactus, about the symmetry, it's good to have it reminded Smile, I tend to forget how important it is, depending on the shape.

I would also rotate the CF by 90° each, to help to prevent from warping.

I don't plan to use infusion polyester, so I think I'll do the way you propose. This stack sounds really good to me (I would have tried with woven glass, though, if I had some).

Will definitely post a picture of the final part, if I succeed Wink !

thanks, again.

J.