EL160 High Temp Epoxy Laminating Resin mould laminating


Author
Message
K.C.C
K.C.C
Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)
Group: Forum Members
Posts: 54, Visits: 117
Hello, I have been working many years with the unimould system but now I going over to the High Temp mould system for the xpreg prepregs . 

I am laminating the mould with 1 layer 100G woven glass than 1 layer 280G woven glass after this I let it set to gell 
han I put 2 layers of 400G woven glass and stop with 1 layer 100G glass to finish.

Are this enough layers for the moulds ? 
And also "why I dont like epoxy " is there a way to not get the air coming up to the high spots in the moulds . 
I make superbike fairings and they got alot of shard , round edges and when the glass and epoxy is just layed down , I dont got any airbubbles but after time the wil show up at high spots . 

This is why I first put the 100G and 280G and leave them to gell first . 
Replies
K.C.C
K.C.C
Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)
Group: Forum Members
Posts: 54, Visits: 117
Tooling seems to work fine ?
I'm making 4 little moulds today again with 1 layer gelcoat 
 pc nice belly from your bike what bike is it ? 

 also noticed to put down the gelcoat I get better results using this type of brush

Thats why I changed to  2 layers gelcoat I wanted first to put down a fine layer with these more stif brushes especially in the sharp corners of the split moulds .
I always did this with the unimould gelcoat so I can get the split corners airbubble free and afte rthat a second layer with a normal brush. 
But I now see my 3 moulds I made of high temp epoxy tooling with 1 layer having some minor air bubbles but no delaminating or my 4 moulds now with  2 layers no airbubbles but delaminating gelcoat so 1 layer it wil bee I think . 

will take some pics later 

Edited 6 Years Ago by K.C.C
Shaneer22
Shaneer22
Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)
Group: Forum Members
Posts: 156, Visits: 14K
K.C.C - 12/27/2019 10:18:17 AM
Tooling seems to work fine ?
I'm making 4 little moulds today again with 1 layer gelcoat 
 pc nice belly from your bike what bike is it ? 

 also noticed to put down the gelcoat I get better results using this type of brush

Thats why I changed to  2 layers gelcoat I wanted first to put down a fine layer with these more stif brushes especially in the sharp corners of the split moulds .
I always did this with the unimould gelcoat so I can get the split corners airbubble free and afte rthat a second layer with a normal brush. 
But I now see my 3 moulds I made of high temp epoxy tooling with 1 layer having some minor air bubbles but no delaminating or my 4 moulds now with  2 layers no airbubbles but delaminating gelcoat so 1 layer it wil bee I think . 

will take some pics later 

I use angled fitchs from brewers paint shop stiffer so easier to use.put the tooling mold is in oven again  to do final post cure.the mold is a lot thinner in carbon it will be interesting how part will come out.will test Monday.

K.C.C
K.C.C
Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)
Group: Forum Members
Posts: 54, Visits: 117
Shaneer22 - 12/27/2019 12:42:21 PM
K.C.C - 12/27/2019 10:18:17 AM
Tooling seems to work fine ?
I'm making 4 little moulds today again with 1 layer gelcoat 
 pc nice belly from your bike what bike is it ? 

 also noticed to put down the gelcoat I get better results using this type of brush

Thats why I changed to  2 layers gelcoat I wanted first to put down a fine layer with these more stif brushes especially in the sharp corners of the split moulds .
I always did this with the unimould gelcoat so I can get the split corners airbubble free and afte rthat a second layer with a normal brush. 
But I now see my 3 moulds I made of high temp epoxy tooling with 1 layer having some minor air bubbles but no delaminating or my 4 moulds now with  2 layers no airbubbles but delaminating gelcoat so 1 layer it wil bee I think . 

will take some pics later 

I use angled fitchs from brewers paint shop stiffer so easier to use.put the tooling mold is in oven again  to do final post cure.the mold is a lot thinner in carbon it will be interesting how part will come out.will test Monday.


just had my el160 laminating resin down on the 1 layer geloat parts.
Only problem I noticed it that on sharp edges the EL160 desolves the gelcoat and you can see the part thru it.
Dont know how big a problim this wil be but had this with the unimould tooling resin also and didn't got any problems  so lets hope this wil work also .
Shaneer22
Shaneer22
Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)
Group: Forum Members
Posts: 156, Visits: 14K
K.C.C - 12/27/2019 12:57:51 PM
Shaneer22 - 12/27/2019 12:42:21 PM
K.C.C - 12/27/2019 10:18:17 AM
Tooling seems to work fine ?
I'm making 4 little moulds today again with 1 layer gelcoat 
 pc nice belly from your bike what bike is it ? 

 also noticed to put down the gelcoat I get better results using this type of brush

Thats why I changed to  2 layers gelcoat I wanted first to put down a fine layer with these more stif brushes especially in the sharp corners of the split moulds .
I always did this with the unimould gelcoat so I can get the split corners airbubble free and afte rthat a second layer with a normal brush. 
But I now see my 3 moulds I made of high temp epoxy tooling with 1 layer having some minor air bubbles but no delaminating or my 4 moulds now with  2 layers no airbubbles but delaminating gelcoat so 1 layer it wil bee I think . 

will take some pics later 

I use angled fitchs from brewers paint shop stiffer so easier to use.put the tooling mold is in oven again  to do final post cure.the mold is a lot thinner in carbon it will be interesting how part will come out.will test Monday.


just had my el160 laminating resin down on the 1 layer geloat parts.
Only problem I noticed it that on sharp edges the EL160 desolves the gelcoat and you can see the part thru it.
Dont know how big a problim this wil be but had this with the unimould tooling resin also and didn't got any problems  so lets hope this wil work also .

Trial and error and testing just laid up this part going to leave it for a day at room temp then cure.useually I bake straight away.

K.C.C
K.C.C
Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)
Group: Forum Members
Posts: 54, Visits: 117
Shaneer22 - 12/27/2019 2:20:23 PM
K.C.C - 12/27/2019 12:57:51 PM
Shaneer22 - 12/27/2019 12:42:21 PM
K.C.C - 12/27/2019 10:18:17 AM
Tooling seems to work fine ?
I'm making 4 little moulds today again with 1 layer gelcoat 
 pc nice belly from your bike what bike is it ? 

 also noticed to put down the gelcoat I get better results using this type of brush

Thats why I changed to  2 layers gelcoat I wanted first to put down a fine layer with these more stif brushes especially in the sharp corners of the split moulds .
I always did this with the unimould gelcoat so I can get the split corners airbubble free and afte rthat a second layer with a normal brush. 
But I now see my 3 moulds I made of high temp epoxy tooling with 1 layer having some minor air bubbles but no delaminating or my 4 moulds now with  2 layers no airbubbles but delaminating gelcoat so 1 layer it wil bee I think . 

will take some pics later 

I use angled fitchs from brewers paint shop stiffer so easier to use.put the tooling mold is in oven again  to do final post cure.the mold is a lot thinner in carbon it will be interesting how part will come out.will test Monday.


just had my el160 laminating resin down on the 1 layer geloat parts.
Only problem I noticed it that on sharp edges the EL160 desolves the gelcoat and you can see the part thru it.
Dont know how big a problim this wil be but had this with the unimould tooling resin also and didn't got any problems  so lets hope this wil work also .

Trial and error and testing just laid up this part going to leave it for a day at room temp then cure.useually I bake straight away.


How did it go ? 
I made 6 little test moulds with 1 layer gelcoat and they came out perfect , post cured them and trimmed all good . 
Had 2 other small moulds with 2 layers waited only 1U30min between first and second layer the gelcoat at arround 20°C room temp and stil when trimming the edges off the moulds delamination . 
Shaneer22
Shaneer22
Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)
Group: Forum Members
Posts: 156, Visits: 14K
K.C.C - 12/30/2019 8:47:20 AM
Shaneer22 - 12/27/2019 2:20:23 PM
K.C.C - 12/27/2019 12:57:51 PM
Shaneer22 - 12/27/2019 12:42:21 PM
K.C.C - 12/27/2019 10:18:17 AM
Tooling seems to work fine ?
I'm making 4 little moulds today again with 1 layer gelcoat 
 pc nice belly from your bike what bike is it ? 

 also noticed to put down the gelcoat I get better results using this type of brush

Thats why I changed to  2 layers gelcoat I wanted first to put down a fine layer with these more stif brushes especially in the sharp corners of the split moulds .
I always did this with the unimould gelcoat so I can get the split corners airbubble free and afte rthat a second layer with a normal brush. 
But I now see my 3 moulds I made of high temp epoxy tooling with 1 layer having some minor air bubbles but no delaminating or my 4 moulds now with  2 layers no airbubbles but delaminating gelcoat so 1 layer it wil bee I think . 

will take some pics later 

I use angled fitchs from brewers paint shop stiffer so easier to use.put the tooling mold is in oven again  to do final post cure.the mold is a lot thinner in carbon it will be interesting how part will come out.will test Monday.


just had my el160 laminating resin down on the 1 layer geloat parts.
Only problem I noticed it that on sharp edges the EL160 desolves the gelcoat and you can see the part thru it.
Dont know how big a problim this wil be but had this with the unimould tooling resin also and didn't got any problems  so lets hope this wil work also .

Trial and error and testing just laid up this part going to leave it for a day at room temp then cure.useually I bake straight away.


How did it go ? 
I made 6 little test moulds with 1 layer gelcoat and they came out perfect , post cured them and trimmed all good . 
Had 2 other small moulds with 2 layers waited only 1U30min between first and second layer the gelcoat at arround 20°C room temp and stil when trimming the edges off the moulds delamination . 

I am out at present will let you no when I get home interesting results.

Shaneer22
Shaneer22
Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)
Group: Forum Members
Posts: 156, Visits: 14K
K.C.C - 12/30/2019 8:47:20 AM
Shaneer22 - 12/27/2019 2:20:23 PM
K.C.C - 12/27/2019 12:57:51 PM
Shaneer22 - 12/27/2019 12:42:21 PM
K.C.C - 12/27/2019 10:18:17 AM
Tooling seems to work fine ?
I'm making 4 little moulds today again with 1 layer gelcoat 
 pc nice belly from your bike what bike is it ? 

 also noticed to put down the gelcoat I get better results using this type of brush

Thats why I changed to  2 layers gelcoat I wanted first to put down a fine layer with these more stif brushes especially in the sharp corners of the split moulds .
I always did this with the unimould gelcoat so I can get the split corners airbubble free and afte rthat a second layer with a normal brush. 
But I now see my 3 moulds I made of high temp epoxy tooling with 1 layer having some minor air bubbles but no delaminating or my 4 moulds now with  2 layers no airbubbles but delaminating gelcoat so 1 layer it wil bee I think . 

will take some pics later 

I use angled fitchs from brewers paint shop stiffer so easier to use.put the tooling mold is in oven again  to do final post cure.the mold is a lot thinner in carbon it will be interesting how part will come out.will test Monday.


just had my el160 laminating resin down on the 1 layer geloat parts.
Only problem I noticed it that on sharp edges the EL160 desolves the gelcoat and you can see the part thru it.
Dont know how big a problim this wil be but had this with the unimould tooling resin also and didn't got any problems  so lets hope this wil work also .

Trial and error and testing just laid up this part going to leave it for a day at room temp then cure.useually I bake straight away.


How did it go ? 
I made 6 little test moulds with 1 layer gelcoat and they came out perfect , post cured them and trimmed all good . 
Had 2 other small moulds with 2 layers waited only 1U30min between first and second layer the gelcoat at arround 20°C room temp and stil when trimming the edges off the moulds delamination . 

First thing sprocket cover made using pre preg tooling.came out near perfect see photo.second part using high temp resin system not so good dry patches.you can't see in photo.extended cure only difference is ramp to 65 and dwell there rather than 70.when I demolded last night pre preg tooling cooled down very quick compared to high temp which retained heat for hours longer due to the thickness of mold which compared to pre preg tooling.iam now going to make pre preg molds from other part to see if part differs.

Shaneer22
Shaneer22
Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)
Group: Forum Members
Posts: 156, Visits: 14K
Shaneer22 - 12/30/2019 3:56:48 PM
K.C.C - 12/30/2019 8:47:20 AM
Shaneer22 - 12/27/2019 2:20:23 PM
K.C.C - 12/27/2019 12:57:51 PM
Shaneer22 - 12/27/2019 12:42:21 PM
K.C.C - 12/27/2019 10:18:17 AM
Tooling seems to work fine ?
I'm making 4 little moulds today again with 1 layer gelcoat 
 pc nice belly from your bike what bike is it ? 

 also noticed to put down the gelcoat I get better results using this type of brush

Thats why I changed to  2 layers gelcoat I wanted first to put down a fine layer with these more stif brushes especially in the sharp corners of the split moulds .
I always did this with the unimould gelcoat so I can get the split corners airbubble free and afte rthat a second layer with a normal brush. 
But I now see my 3 moulds I made of high temp epoxy tooling with 1 layer having some minor air bubbles but no delaminating or my 4 moulds now with  2 layers no airbubbles but delaminating gelcoat so 1 layer it wil bee I think . 

will take some pics later 

I use angled fitchs from brewers paint shop stiffer so easier to use.put the tooling mold is in oven again  to do final post cure.the mold is a lot thinner in carbon it will be interesting how part will come out.will test Monday.


just had my el160 laminating resin down on the 1 layer geloat parts.
Only problem I noticed it that on sharp edges the EL160 desolves the gelcoat and you can see the part thru it.
Dont know how big a problim this wil be but had this with the unimould tooling resin also and didn't got any problems  so lets hope this wil work also .

Trial and error and testing just laid up this part going to leave it for a day at room temp then cure.useually I bake straight away.


How did it go ? 
I made 6 little test moulds with 1 layer gelcoat and they came out perfect , post cured them and trimmed all good . 
Had 2 other small moulds with 2 layers waited only 1U30min between first and second layer the gelcoat at arround 20°C room temp and stil when trimming the edges off the moulds delamination . 

First thing sprocket cover made using pre preg tooling.came out near perfect see photo.second part using high temp resin system not so good dry patches.you can't see in photo.extended cure only difference is ramp to 65 and dwell there rather than 70.when I demolded last night pre preg tooling cooled down very quick compared to high temp which retained heat for hours longer due to the thickness of mold which compared to pre preg tooling.iam now going to make pre preg molds from other part to see if part differs.



GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
oekmont - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
             What post cure cycles do you use ?
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
                         Fairing for my bike.
Shaneer22 - 6 Years Ago
                             Just demolded tooling.
Shaneer22 - 6 Years Ago
carbon man - 5 Years Ago
K.C.C - 5 Years Ago
carbon man - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
                             I am out at present will let you no when I get home interesting results.
Shaneer22 - 6 Years Ago
Shaneer22 - 6 Years Ago
                                 + x [quote] [b] Shaneer22 - 12/30/2019 3:56:48 PM [/b] + x [quote] [b]...
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
             Your using x preg.
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
Warren (Staff) - 5 Years Ago
K.C.C - 5 Years Ago
Warren (Staff) - 5 Years Ago
kip - 5 Years Ago
Warren (Staff) - 5 Years Ago
kip - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
                 Maybe
benji82 - 5 Years Ago
                     I make these ones
K.C.C - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
     some moulds
K.C.C - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
             Can you send a pic pls :D
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
K.C.C - 5 Years Ago
Warren (Staff) - 5 Years Ago
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
             It just looks good thats why :D
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
Hanaldo - 5 Years Ago
                 ok thnx
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
Hanaldo - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
Hanaldo - 5 Years Ago
Hanaldo - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
Hanaldo - 5 Years Ago
K.C.C - 5 Years Ago