Hello,

I have a small question...I do not have access to  a good oven for out-of-autoclave pre-preg (at least not good enough that the cycles are accurate), but I do have access to a sterilizing autoclave...

Sorry for the naive questions, but is such an autoclave OK for pre-preg ? Do you need to keep a vacuum system when using an autoclave despite the fact that there is high pressure in the autoclave itself ? Is moisture a problem (or it's OK but the part must then be put in a protective bag) ? Can someone give me a link to an autoclave protocol (temperature, time, pressure) for the use of the pre-preg in such system ? I don't think there is much indicated on the easycomposite website on that.

Thank you !!

cpkielycua
cpkielycua
Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)
Group: Forum Members
Posts: 29, Visits: 285
Can anyone recommend a small composites autoclave?  2ft x 2ft x 3ft in size?

To answer your question:

Sterilizing autoclaves generally speaking use heat rather than pressure.  You need low heat and some pressure.  
I would not recommend a sterilizing autoclave for composites.  Yes, you would need to keep the vacuum on the entire time for imperfect vacuum bags, but also for outgassing of the part and any moisture.  Obviously you do not want to put the vacuum pump in the oven.  For the spec, go to the product page and download the doc.
scottracing
scottracing
Supreme Being (6.2K reputation)Supreme Being (6.2K reputation)Supreme Being (6.2K reputation)Supreme Being (6.2K reputation)Supreme Being (6.2K reputation)Supreme Being (6.2K reputation)Supreme Being (6.2K reputation)Supreme Being (6.2K reputation)Supreme Being (6.2K reputation)
Group: Forum Members
Posts: 460, Visits: 5.2K
Get yourself one of the rodwell autoclaves you can buy or lease them. Ive used one a few times now for small cures, simple to use and ideal for the hobbysist up to the pro shop.

http://www.rodwell-autoclave.com/autoclave/dwell-pro-280/


Damien
Damien
Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)
Group: Forum Members
Posts: 32, Visits: 132
scottracing - 4/5/2019 1:45:20 PM
Get yourself one of the rodwell autoclaves you can buy or lease them. Ive used one a few times now for small cures, simple to use and ideal for the hobbysist up to the pro shop.

http://www.rodwell-autoclave.com/autoclave/dwell-pro-280/



Thanks !

Rakesh Verma
Rakesh Verma
Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)
Group: Forum Members
Posts: 6, Visits: 50
cpkielycua - 3/9/2019 8:43:38 PM
Can anyone recommend a small composites autoclave?  2ft x 2ft x 3ft in size?

To answer your question:

Sterilizing autoclaves generally speaking use heat rather than pressure.  You need low heat and some pressure.  
I would not recommend a sterilizing autoclave for composites.  Yes, you would need to keep the vacuum on the entire time for imperfect vacuum bags, but also for outgassing of the part and any moisture.  Obviously you do not want to put the vacuum pump in the oven.  For the spec, go to the product page and download the doc.

If you are still looking for Autoclave Contact +8613861177443 (WhatsApp) or Direct call 


Rakesh Verma
+8613861177443
vermachina@gmail.com



Steve Broad
Steve Broad
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
scottracing - 4/5/2019 1:45:20 PM
Get yourself one of the rodwell autoclaves you can buy or lease them. Ive used one a few times now for small cures, simple to use and ideal for the hobbysist up to the pro shop.

http://www.rodwell-autoclave.com/autoclave/dwell-pro-280/


Maybe for well heeled hobbyists :-)

Rakesh Verma
Rakesh Verma
Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)
Group: Forum Members
Posts: 6, Visits: 50
Damien Coudreuse - 2/6/2019 1:02:42 PM
[quote]
Damien Coudreuse - 2/6/2019 1:02:42 PM
Hello,

I have a small question...I do not have access to  a good oven for out-of-autoclave pre-preg (at least not good enough that the cycles are accurate), but I do have access to a sterilizing autoclave...

Sorry for the naive questions, but is such an autoclave OK for pre-preg ? Do you need to keep a vacuum system when using an autoclave despite the fact that there is high pressure in the autoclave itself ? Is moisture a problem (or it's OK but the part must then be put in a protective bag) ? Can someone give me a link to an autoclave protocol (temperature, time, pressure) for the use of the pre-preg in such system ? I don't think there is much indicated on the easycomposite website on that.

Thank you !!


https://xirtue.net/composite-autoclave/


Rakesh Verma
+8613861177443
vermachina@gmail.com



GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search