Hi.

Ok happened my fault.
I did not steer resin enough or used wrong ratio, after 5 days still have few soft spots on my part.
What can I do to fix it?
Or it cannot be fixed and i have to scrap the part.
Part das not need to look nice it is bottom part of my bonnet.

 
Reply
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Initially try and use some heat to see if it will cook off.  Is it right through or just on the surface? Surface you can just gouge it off and recoat.

Patches of poorly cured resin are not usually a mixing ratio issue  -  the whole lot would likely be soft if it is.  Patches is normally poor mixing, either you didn't spend enough time mixing or did not mix it properly.  Sometimes it can be the last dregs from the mixing bucket too but that can be avoided by mixing, then pouring into a jug or similar to infuse from.


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search