+x Warren (Staff) - 2/8/2019 11:19:33 AM24inhg is a bit low and could well be the cause of the issues you have - or at least part of it..I presume the dry patches are at the vacuum line end of the mould? You may also find on such a small sheet, the infusion flows too quickly meaning it skips over the surface without enough time to soak in fully. You can help this by throttling the resin feed with a line clamp to slow things down.