Dear sir,

I did resin infusion process for 175 x 150 mm flat plate in glass and carbon fabric. But I faced huge problem. Here i attached the photos. Kindly help me to solve this problem.

I used Vacuum pump, specification is  630 mm of Hg (or )  24 in Hg. and its dry vacuum pump single stage. Is sufficient to do the infusion process?

Some times plate get good finishing. Some times problem will come (See the photos)
Replies
Lester Populaire
L
Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
To me this does not look like a pump/vacuum issue, but rather something that can be solved with the right infusion setup. Can you provide a picture of the opposite side of the part with the flow media?

It might already be enough to just heat the vacuum bag with a heat gun along the sides, so it can conform better to the edge of the fabric to avoid race tracking.

cheers, Lester
Balakrishnan Seeni
Balakrishnan Seeni
Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)
Group: Forum Members
Posts: 3, Visits: 5
Lester Populaire - 2/8/2019 11:34:43 AM
To me this does not look like a pump/vacuum issue, but rather something that can be solved with the right infusion setup. Can you provide a picture of the opposite side of the part with the flow media?

It might already be enough to just heat the vacuum bag with a heat gun along the sides, so it can conform better to the edge of the fabric to avoid race tracking.

cheers, Lester

Thank You for valuable reply Lester..  here i attached the opposite side of the part. This side is fully impregnated.  help me to solve the above problem 

Lester Populaire
L
Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
Balakrishnan Seeni - 3/3/2019 2:00:02 PM
Lester Populaire - 2/8/2019 11:34:43 AM
To me this does not look like a pump/vacuum issue, but rather something that can be solved with the right infusion setup. Can you provide a picture of the opposite side of the part with the flow media?

It might already be enough to just heat the vacuum bag with a heat gun along the sides, so it can conform better to the edge of the fabric to avoid race tracking.

cheers, Lester

Thank You for valuable reply Lester..  here i attached the opposite side of the part. This side is fully impregnated.  help me to solve the above problem 

I meant a picture of the bagged part with the flow media and vacuum line. A sketch would do if you don't have a picture...