Balakrishnan Seeni - 2/8/2019 10:43:26 AM
Dear sir,

I did resin infusion process for 175 x 150 mm flat plate in glass and carbon fabric. But I faced huge problem. Here i attached the photos. Kindly help me to solve this problem.

I used Vacuum pump, specification is  630 mm of Hg (or )  24 in Hg. and its dry vacuum pump single stage. Is sufficient to do the infusion process?

Some times plate get good finishing. Some times problem will come (See the photos)

Looks like you demoulded to early to me... you're talking of the problems on the bottom of your plate right? looks like resin was still sticking to the mould? You are using epoxy right? make sure it's fully cured at 25°C preferably even with a postcure and make sure to wait 48 hours to be sure before demoulding 


Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




Lester Populaire
L
Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
Balakrishnan Seeni - 3/3/2019 2:00:02 PM
Lester Populaire - 2/8/2019 11:34:43 AM
To me this does not look like a pump/vacuum issue, but rather something that can be solved with the right infusion setup. Can you provide a picture of the opposite side of the part with the flow media?

It might already be enough to just heat the vacuum bag with a heat gun along the sides, so it can conform better to the edge of the fabric to avoid race tracking.

cheers, Lester

Thank You for valuable reply Lester..  here i attached the opposite side of the part. This side is fully impregnated.  help me to solve the above problem 

I meant a picture of the bagged part with the flow media and vacuum line. A sketch would do if you don't have a picture...

Balakrishnan Seeni
Balakrishnan Seeni
Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)
Group: Forum Members
Posts: 3, Visits: 5
Lester Populaire - 2/8/2019 11:34:43 AM
To me this does not look like a pump/vacuum issue, but rather something that can be solved with the right infusion setup. Can you provide a picture of the opposite side of the part with the flow media?

It might already be enough to just heat the vacuum bag with a heat gun along the sides, so it can conform better to the edge of the fabric to avoid race tracking.

cheers, Lester

Thank You for valuable reply Lester..  here i attached the opposite side of the part. This side is fully impregnated.  help me to solve the above problem 

Balakrishnan Seeni
Balakrishnan Seeni
Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)
Group: Forum Members
Posts: 3, Visits: 5
Warren (Staff) - 2/8/2019 11:19:33 AM
24inhg is a bit low and could well be the cause of the issues you have - or at least part of it..

I presume the dry patches are at the vacuum line end of the mould?  You may also find on such a small sheet, the infusion flows too quickly meaning it skips over the surface without enough time to soak in fully.  You can help this by throttling the resin feed with a line clamp to slow things down.

Thank you for your reply

Lester Populaire
L
Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
To me this does not look like a pump/vacuum issue, but rather something that can be solved with the right infusion setup. Can you provide a picture of the opposite side of the part with the flow media?

It might already be enough to just heat the vacuum bag with a heat gun along the sides, so it can conform better to the edge of the fabric to avoid race tracking.

cheers, Lester
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
24inhg is a bit low and could well be the cause of the issues you have - or at least part of it..

I presume the dry patches are at the vacuum line end of the mould?  You may also find on such a small sheet, the infusion flows too quickly meaning it skips over the surface without enough time to soak in fully.  You can help this by throttling the resin feed with a line clamp to slow things down.


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Balakrishnan Seeni
Balakrishnan Seeni
Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)Junior Member (21 reputation)
Group: Forum Members
Posts: 3, Visits: 5
Dear sir,

I did resin infusion process for 175 x 150 mm flat plate in glass and carbon fabric. But I faced huge problem. Here i attached the photos. Kindly help me to solve this problem.

I used Vacuum pump, specification is  630 mm of Hg (or )  24 in Hg. and its dry vacuum pump single stage. Is sufficient to do the infusion process?

Some times plate get good finishing. Some times problem will come (See the photos)