Wiring in the the part?


Author
Message
Classicarbon
C
Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)
Group: Forum Members
Posts: 86, Visits: 639
I'm before making my rear engine lid. As the lid got place for rear number plate I was thinking if I could insert wireing underneath the CF bonnet. 
I know normally heating in aerospace is installed inside the composite part and on the ends are plugs.
Is it possible just to use normal wires? But then it will have to come out through the bag to not being soaked with resin.
Distance I'm thinking of is with red line.


Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
I wouldn't, you're making life very difficult for yourself, especially for infusion. Why do you want to do it?
Classicarbon
C
Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)
Group: Forum Members
Posts: 86, Visits: 639
Hanaldo - 2/1/2020 10:00:45 AM
I wouldn't, you're making life very difficult for yourself, especially for infusion. Why do you want to do it?

I building aerospace.seals for living.Build next door which is part of same company they do air intakes for helicopters which are heated.So I thought the wireing could be done for electrics.Different is they do prepreg and I doing infiusion.I could have cables integrated in the part.

Lester Populaire
L
Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
I built race car parts with integrated electronics and cables in infusion and prepreg. It is certainly possible, but for your application i cannot see the advantage. I would rather integrate a cable channel so you have a neat solution to hide the cables, but everything remains independent so you can switch things out.
Classicarbon
C
Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)
Group: Forum Members
Posts: 86, Visits: 639
Lester Populaire - 2/2/2020 7:32:22 AM
I built race car parts with integrated electronics and cables in infusion and prepreg. It is certainly possible, but for your application i cannot see the advantage. I would rather integrate a cable channel so you have a neat solution to hide the cables, but everything remains independent so you can switch things out.

Ooo that's great idea. 

f1rob
f1rob
Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)
Group: Forum Members
Posts: 237, Visits: 4.8K
Lot of the f1 floors have silicone cable bonded in the laminate.
Pulled out after cure an the wiring/pressure taps then threaded through