Yeh, it's just not enough resin. And given the size of your samples, that's not surprising - infusing small pieces with proper infusion resin can be tricky, as the resin often just flows super quick over the back and doesnt have time to wet out the surface properly. With bigger infusions this solves itself as the resin doesnt flow as quickly, but with smaller infusions it can be helpful to use a higher viscosity resin (max 550cps), or just use a hose clamp to throttle the flow to about an inch per minute.
|