Group: Forum Members
Posts: 550,
Visits: 27K
|
My setup: -2 Layers of 160g twill glass. Keep in mind, that this will likely have a higher flow resistance than 1 layer of 240g twill carbon, due to it's finer weave. Nur mit that mich, that oh really matters Herr. -On top of that stripes (12cm wide) of lantor coremat, soric lrc 1,5mm and 3mm and 3d pet core 3mm, as well as a 12cm stripe without a sandwich core -2 layers of 160g twill glass -peel ply -flow Media (a heavy one) over one half -a spiral tube along the middle. Placed on top of the stack -bagging film, placed without wrinkles, as they can be an even faster flow path than flow mesh -glass plate heated to 30°c -resin: up textiles standard infusion resin, medium hardener, heated to 30°c
|