Problem when I apply gelcoat to the mould


Author
Message
67redrocket
67redrocket
Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)
Group: Forum Members
Posts: 49, Visits: 486
I have a mould that i cleaned with the mould cleaner. Then I applyed easy lease, apx 7 coats. 

i used a brush to apply the G50 gelcoat. I could not get a even coat, because i got holes in the coat. Looked like the mould had been contaminated by chemicals, but iam shure it isnt. The gelcoat cured for a couple of hours before i took i of. Iam cleaning again with the mould cleaner but it dont seem to evaporise like it i remember it does. It still look like the mould is contaminated. 

Any ideas?
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
It is contaminated; by the release agent. That's a common issue with chemical release agents, they are too high slip for brushing gelcoats onto. You can get it to work when sprayed, but brushing is harder. 

It will help to apply 2-3 coats of silicone free release wax AFTER you have reapplied the Easylease. This will raise the surface tension slightly and make it a bit easier, though you will still have a bit of trouble. 
alex.mc
alex.mc
Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)
Group: Forum Members
Posts: 18, Visits: 52
This is the age old problem! The better the release, the more likely it is to create such a high surface tension that your resin/gel will shrink back.

PVA is neutral, and the GC50 will sit nicely on it. But you will have the same problem getting the PVA on the chemical release.

Waxing over chemical release will help as mentioned, but you are mixing products which can be difficult!

Spraying the GC50 will work, with a bit of effort in the application.
I spray the GC50 in a fine mist first and then leave it 3 mins, then I spray again and it's much better, another 3/5 mins and the last coat goes on and usually it's now covering completely. It's as if the first layer gasses off it's volatiles, and "settles" a bit. The second coat continues this... and the 3/4th ones are now going down on a "settled" base.

That's what I do, I'd love to hear other techniques though.
67redrocket
67redrocket
Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)Supreme Being (415 reputation)
Group: Forum Members
Posts: 49, Visits: 486
I did a new try. Cleaned the mold with the EC mouldcleaner. Then three coats of easy lease and then three coats of megauliars mould wax nr. 8. 

Same thing happend. lots of holes in the gel coat. 

Does the mould cleaner remove the easylease?
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Yes mould cleaner will remove the Easylease. You shouldn't need to use mould cleaner anyway, there's no issue with what is on your mould. The issue is that you are trying to apply a liquid to a surface with very little energy, so the liquid adheres to itself easier than it adheres to the surface. This causes the droplets of liquid to form the shape that requires the least amount of surface area, a sphere or 'bead'. 

There's no easy solution for this as it's a simple physics issue. The best solution is to spray the gelcoat. If you have an area where you can spray, borrow or buy a compressor and a cheap HVLP gun (preferably with a 2.0-2.5mm tip). Then the technique that Alex described works perfectly and is the best way of applying an in mould coating. 