Epoxy needs to cure at around 20 degreesfor its full cure cycle. Anything less and it can ‘go off the boil’ and end upnever going off properly. As the weather get colder we get many calls frompeople with problems with resin curing, in most cases it's because the workingenvironment is colder that they thought.
Excess humidity and cold combined can be a killer for epoxy curing meaning it sometimes won't cure at all! To rectify that it will need curing well above 20c in a dry environment to drive out the moisture. Even then it might need a recoat to get rid of a tacky surface.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|