I have laminated a carbon frame tube using 3k 2x2 and unidirectional carbon, Using vacuum bagging! wrinkles have appeared after demould and i wondered why , is the bagging too loose , any advice or tips greatly appreciated!
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
do you have some pictures? are you talking about the wrinkles of your bag? or did the part came out perfect and then started to wrinkle?

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




whereismillar
whereismillar
Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)
Group: Forum Members
Posts: 10, Visits: 31
Hi mathieu

No the carbon itself is wrinkled after removing everything post cure! where the vacuum bag itself was wrinkled when using the pump and curing
no pictures yet but will post some tomorrow
before bagging the carbon , peel ply , perforated film, and breather cloth were carefully applied!

.
Edited 11 Years Ago by whereismillar
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
Ok, I'll wait for some images Smile

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




ChrisR
ChrisR
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 363, Visits: 3K
How long after the initial cure did you demould? Some epoxies require an on mould postcure and others can be post cured off the mould. If it distorted during the post cure it sounds like either the resin wasn't cured enough before initial demould or it softened during the postcure and the forces from the vac bag have caused the distortion.

Pictures should tell all but that was my initial thoughts on it
whereismillar
whereismillar
Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)
Group: Forum Members
Posts: 10, Visits: 31
hi chris 
I actually waited 2 days before demolding
the wrinkles in the carbon match the initial wrinkles that formed 
in the bagging film when turning on the pump, i waited till the resin left in the mixing pot  was solid before turning off the pump
curing was done in a box at roughly 35 degrees for the whole time the pump was on,



cheers!





http://www.talkcomposites.com/Uploads/Images/6d140706-31f9-4d62-9342-ce8a.JPG
Edited 11 Years Ago by whereismillar
ajb100
ajb100
Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)
Group: Forum Members
Posts: 346, Visits: 4.4K
How thick is the layup? When you vac bag tubes, the OD shrinks under the pressure and you can can folds in the carbon. It is increased with thickness as you put it on tight, apply vac and all the layers compress creating the wrinkle
whereismillar
whereismillar
Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)Supreme Being (78 reputation)
Group: Forum Members
Posts: 10, Visits: 31
i used  0.10 x2, and one of 0.20 carbon cloth 3 layers in total!

I was led to believe that vacuum bagging a repair this way was the best way to go ?
Edited 11 Years Ago by whereismillar
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
like above if you are making tubes and the CF isnt tight against the tube it will start to wrinkle, It's very hard to get it right, adding peelply to pull everything tight can help, or a piece of vacuumbag

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




ChrisR
ChrisR
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 363, Visits: 3K
It might be better to try a shrinkwrap tape carefully wrapped around the layup rather than vac bag.