Group: Administrators
Posts: 2.5K,
Visits: 8.5K
|
We would very strongly advise against trying to use GC50 with a polyester resin. The GC50 has been uniquely formulated to be epoxy compatible in its cured surface finish by being tack free (as well as the formulation). If you tried to use a polyester resin on the back of a cured GC50, assuming there was no reaction of one against the other, you would find the gelcoat would delaminate very badly, ruining the part.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|