jamesw
jamesw
Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)
Group: Forum Members
Posts: 61, Visits: 558
My third infusion - and finally this one pulled straight from the mold and only needed a quick polish and trim to look like this!

Spraying  GC50 into the mould with the G100 gel spray gun has transformed my pieces (I was pinhole free on infusion 2 but was having carbon exposed at the surface)

There has been a lot of discussion about problems brushing GC50 - I have to advise just getting the correct kit and spraying it...

http://i.imgur.com/ObrGYdV.jpg
Edited 12 Years Ago by jamesw
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
Excellent work Smile I have been banging on about the benefits of GC50 for a while now (spray application) 
UV protection, hard glass like finish and acts like a spray tack for the first surface layer (if you get the timing right) What is there not to like BigGrin

Regards Warren

Carbon Copies Ltd
Jess8bit
Jess8bit
Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)
Group: Forum Members
Posts: 133, Visits: 566
Great Job James !

Could you share about the air compressor you used with the spray gun ? (model or spec if possible) I'm close to buy mine, but still hesitating about the tank volume (would 100 liters be enough for spraying a bonnet ?)

thanks a lot Smile
J
jamesw
jamesw
Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)
Group: Forum Members
Posts: 61, Visits: 558
Not huge - 3hp with 50l reservoir - just about keeps up... Hasn't given me any problems spraying parts as large as a bonnet...

Warren - re: getting a tack, I must have left it too late as no amount of spray acetone would generate tack - I was worried about going in with the cloth too early and ruining the finish....
Jess8bit
Jess8bit
Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)Supreme Being (843 reputation)
Group: Forum Members
Posts: 133, Visits: 566
Thanxx for your quick answer w00t
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
It takes a bit of practice to get the timing rightWink in my workshop it's about three hours. I test an area around the flange, if you can feel the tack on your glove without the gelcoat actually sticking to it then you are good to goSmile If you get any large blobs/drips ( easily done ) in the gelcoat then just let it completely cure (overnight) then just flat them back with 1200's (dry)

Regards Warren

Carbon Copies Ltd
prsw
prsw
Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)
Group: Forum Members
Posts: 112, Visits: 1K
And then use the acetone trick to tack the first layer on the fully cured GC50?
(wtf is up with quoting a post, sorry for the mess)

wozza (12/05/2013)
It takes a bit of practice to get the timing rightWink in my workshop it's about three hours. I test an area around the flange, if you can feel the tack on your glove without the gelcoat actually sticking to it then you are good to goSmile If you get any large blobs/drips ( easily done ) in the gelcoat then just let it completely cure (overnight) then just flat them back with 1200's (dry)
Edited 12 Years Ago by prsw
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Acetone doesnt work on GC50 anymore.  The formulation has changed slightly since our bonnet video was filmed.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
jamesw
jamesw
Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)Supreme Being (497 reputation)
Group: Forum Members
Posts: 61, Visits: 558
Aha, that would explain it!

Does the new formulation offer any other benefits/changes?  What would you recommend for a quick 1st layer spray tack? Aerofix 2? I have used meths+infusion resin before but it takes a heck of a long time to cure to a tack...

James
prsw
prsw
Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)
Group: Forum Members
Posts: 112, Visits: 1K
ok, to bad.
then I will hold on tight to the bottle I got.

Warren (Staff) (14/05/2013)
Acetone doesnt work on GC50 anymore.  The formulation has changed slightly since our bonnet video was filmed.



http://motoform.blogspot.se

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search