From the XC110 datasheet,

CURED MECHANICAL PROPERTIES
Tests performed on XC110-C331T2-210(1250) laminate cured out-ofautoclave
Property Test Standard Units Result
Compressive strength BS EN ISO 14126 : 1999 MPa 483
Tensile strength BS EN ISO 527-4 : 1997 MPa 521
Tensile modulus BS EN ISO 527-4 : 1997 GPa 55.1
Flexural strength BS EN ISO 14125 : 1998 MPa 777
Flexural modulus BS EN ISO 14125 : 1998 GPa 46.7
Interlaminar shear strength BS EN 2563 : 1997 MPa 64.7
Tg Onset (DMA) ASTM 1-0003 Issue 3 °C 121
Tg Peak (DMA) ASTM 1-0003 Issue 3 °C 135

I understand the standards relating to the tests are as specified. Can I have further information (ie. thickness, number of ply(s), method of cure, cure temp & duration, etc..) regarding the specimens sent for these tests?
Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
We do not have specific test token lay up schedule available.  The test token sizes are specified in each BS/ISO standard and the lay up will be as required to meet the required thickness.

This is why the actual data is presented in units that are specifically dimensionless so they can be used for most situations.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search