Yes it went well vaccume wise all the way through thanks everyone 

I had a few problems with the part tho like it looks like it could of been a little more resin rich its all coverd fine but it just looks like it could do with a little more. I used mti on this so I just stopped when it stopped drinkin resin.any ideas?
 I have got normal spiral hose but I'm using mti while I learn 
And secondly I had a few tiny overhangs on the corners of the mould which I didn't notice  and it broke tiny bits off the corners because I didn't get east lease in there enough I think.
Iv sanded the over hangs down now
carbonfibreworks
carbonfibreworks
Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
Jdmleesy (04/02/2014)
Ok so iv just bagged up the mould and I think its worked.
iv tried abit of everyone's advise iv enveloped the part which seemed so much easier to make sure there's no wrinkles as I take the protective tape off the tape and iv put peel ply on every part of the mesh that's cut.so iv now pulled vac onit and iv got to 29hg better than I had b4 and when I turned off the pump I couldn't hear one leak  iv just gotta do a drop test now but I got a good feelin 


Good luck Smile
Chris

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
Jdmleesy
Jdmleesy
Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)
Group: Forum Members
Posts: 39, Visits: 380
Ok so iv just bagged up the mould and I think its worked.
iv tried abit of everyone's advise iv enveloped the part which seemed so much easier to make sure there's no wrinkles as I take the protective tape off the tape and iv put peel ply on every part of the mesh that's cut.so iv now pulled vac onit and iv got to 29hg better than I had b4 and when I turned off the pump I couldn't hear one leak  iv just gotta do a drop test now but I got a good feelin 
Jdmleesy
Jdmleesy
Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)
Group: Forum Members
Posts: 39, Visits: 380
I will defo do that Fred thank you although it didn't look like it had pierced it there b4 but it was only a tiny leak so I could if missed it i suppose.I'm just prepping the mould up ready to give it another go tomorrow hopefully.
Do u guys envelope it aswel or use the pleat method because I don't know if I messed up on the gumtape b4 but I was so carful
ajb100
ajb100
Supreme Being (4.4K reputation)Supreme Being (4.4K reputation)Supreme Being (4.4K reputation)Supreme Being (4.4K reputation)Supreme Being (4.4K reputation)Supreme Being (4.4K reputation)Supreme Being (4.4K reputation)Supreme Being (4.4K reputation)Supreme Being (4.4K reputation)
Group: Forum Members
Posts: 346, Visits: 4.4K
Have to agree with Fred, the white plastic infusion mesh is a paint to get to form to a mould and the edges punctured the bag. I went for a short time wrapping the edges in masking tape until I started using a different mesh and not had any problems since
fgayford
fgayford
Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
Jdmleesy (31/01/2014)
Thanks everyone il give it all a go tomorrow 



In my experience the cause of the leak was ALWAYS the same! It was the infusion mesh flow media!
Any where you have a cut edge in the bag of the flow media is sharp. If you picture it as the sharp edge of a chain link fence you can imagine how easily it will puncture the bag. To solve this problem I simple cut strips of peel ply ( just 2 inches wide) and place them over EVERY single cut line of the flow media! I have NEVER had a leak since and I do a lot of infusion. Before I did this technic I NEVER had a perfectly sealed bag, and I thought it was impossible to have one.
Try it and you will become a believer.
Hope this helps.
Fred
 
Jdmleesy
Jdmleesy
Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)
Group: Forum Members
Posts: 39, Visits: 380
Thanks everyone il give it all a go tomorrow 
carbonfibreworks
carbonfibreworks
Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)Supreme Being (3.8K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
Create a bag using your bagging film/ tape and and insert the mould into the bag.
Chris
carbonfibreworks .co.uk

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
Dravis
Dravis
Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
Cut out a two sheets of bag-film quite a bit larger than the whole mold..   put one on the table top, prepped mold with all things in (CF, peel-ply, mesh, silicone hose holders and infusion spreaders)

Gum around entire edge ,CAREFULLY BigGrin   !

Take the protection tape of the gum strip as you go along putting the top sheet of bagging film down, to avoit getting creases (those are in my experience the sinner in 99 % of all bagging leaks)

If youre worried about sharp points on the outside of your mold, then put it down on af layer of breather cloth...

That's it ... really...

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
Jdmleesy
Jdmleesy
Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)Supreme Being (435 reputation)
Group: Forum Members
Posts: 39, Visits: 380
What's the easiest way to envelope it 
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search