Group: Forum Members
Posts: 135,
Visits: 1.6K
|
I think the answer is simple, he has already explained that he did not mix the separate parts before mixing them together, so he was skimming the top off a part, which cured fast, and the sludge went into the second, which hardly cured.
Get new resin, shake/stir the individual containers, and then mix correctly 50/50.
A friend mixes this on large scale, 30kg containers, and he stirs part A + B separately with a drill and stirring attachment.
cheers
|