We leave our pre-preg items on the vacuum pump throughout the cure process. No reason not to really. With pre-preg if there is a very slight leak you can get away with it if its on the pump.
Generally we dont have many burst bags and even slight leaks usually seal up once in the oven. Unless you are unlucky and puncture the bag, most leaks are around the gum tape or rarely connector.