For such a large infusion, I'd be tempted to use infusion mesh everywhere, just because for a few pounds in cost, you have peace of mind that you know you won't have resin flow issues.
You will need some mesh to bridge the edges that have no Soric.
Soric as a flow media is slightly slower than mesh so for such a large part, having mesh might be a better idea. You can always slow down the resin flow by restricting the feed line, however if its too slow there is little you can do!
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|