Group: Forum Members
Posts: 2.5K,
Visits: 28K
|
I try to avoid using peel ply on things I want to refinish. The texture it applies is quite deep, and can be like trying to recover the appearance from 40 grit scratches. It can still be visible even if you bury it in 20 layers of resin.
I would do the same process using either a shrink wrap, or just a non-perforated release film. You will still squeeze resin out if you apply tension while wrapping, but you won't get the textured finish so it's often a pretty simple and quick job of sanding out the ridges from the edges of the film with a 180 grit paper, and then a single coat of resin can be enough to get a great finish.
|