EL160 High Temp Epoxy Laminating Resin mould laminating


Author
Message
K.C.C
K.C.C
Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)
Group: Forum Members
Posts: 54, Visits: 117
Hello, I have been working many years with the unimould system but now I going over to the High Temp mould system for the xpreg prepregs . 

I am laminating the mould with 1 layer 100G woven glass than 1 layer 280G woven glass after this I let it set to gell 
han I put 2 layers of 400G woven glass and stop with 1 layer 100G glass to finish.

Are this enough layers for the moulds ? 
And also "why I dont like epoxy " is there a way to not get the air coming up to the high spots in the moulds . 
I make superbike fairings and they got alot of shard , round edges and when the glass and epoxy is just layed down , I dont got any airbubbles but after time the wil show up at high spots . 

This is why I first put the 100G and 280G and leave them to gell first . 
Replies
K.C.C
K.C.C
Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)Supreme Being (393 reputation)
Group: Forum Members
Posts: 54, Visits: 117
Lester Populaire - 11/10/2020 9:14:41 AM
K.C.C - 11/10/2020 8:59:55 AM
Lester Populaire - 11/10/2020 8:17:50 AM
That is probably because of the shrinking of the big resin accumulation in the inside corners where the flanges start. As there is are no fibres there it won't make a difference whether you use carbon or glass...

I assume the gap is closing once you bolt them together?

The shrinking is more on the edges on the part itself and some on the flanges. I need to pull each side "open" to get the bolts in there.
Yes I can stil bolt them together with force so it would be possible to make the parts.
Maybee its the postcure cycle I use my max temp is 125°C
I now bolthed them back together and put them in the kitchen oven for 2H at 135°C .
My cure cycles is 20° 1H ramp 1°/min to 30° hold 1H and so on until 125°C and let cool over night
With othe rparts that got more structures in them I dont got the warping .
same cure cycle etc verry little gap when hold them together

My post cure cycle (different resin system tho) is a lot slower with 0.3°C/min and then a 10h at temp, and then again slow-ish ramp down.
This is what was on the datasheet.
The recommended post-cure cycle (above) calls for a temperature ramp
from 50°C to 135°C. If a temperature controller with programmable ramp
rate is not available then the oven temperature can be increased by 12°C
every 2hours until 135°C is reached.
Problem was that my heater in the oven is build for only 80°C and I boosted it out thil I could get to 125°C and the ramp takes really long the higher the temp is going.
Wil need to add heat elements i nthe oven .
But would this warping be caused by cure or resin build up ?

Lester Populaire
L
Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
K.C.C - 11/10/2020 10:36:16 AM
Lester Populaire - 11/10/2020 9:14:41 AM
K.C.C - 11/10/2020 8:59:55 AM
Lester Populaire - 11/10/2020 8:17:50 AM
That is probably because of the shrinking of the big resin accumulation in the inside corners where the flanges start. As there is are no fibres there it won't make a difference whether you use carbon or glass...

I assume the gap is closing once you bolt them together?

The shrinking is more on the edges on the part itself and some on the flanges. I need to pull each side "open" to get the bolts in there.
Yes I can stil bolt them together with force so it would be possible to make the parts.
Maybee its the postcure cycle I use my max temp is 125°C
I now bolthed them back together and put them in the kitchen oven for 2H at 135°C .
My cure cycles is 20° 1H ramp 1°/min to 30° hold 1H and so on until 125°C and let cool over night
With othe rparts that got more structures in them I dont got the warping .
same cure cycle etc verry little gap when hold them together

My post cure cycle (different resin system tho) is a lot slower with 0.3°C/min and then a 10h at temp, and then again slow-ish ramp down.
This is what was on the datasheet.
The recommended post-cure cycle (above) calls for a temperature ramp
from 50°C to 135°C. If a temperature controller with programmable ramp
rate is not available then the oven temperature can be increased by 12°C
every 2hours until 135°C is reached.
Problem was that my heater in the oven is build for only 80°C and I boosted it out thil I could get to 125°C and the ramp takes really long the higher the temp is going.
Wil need to add heat elements i nthe oven .
But would this warping be caused by cure or resin build up ?

My gut feeling sais it is a little bit of both but it is hard to say and there are other people on here who have more experience with split moulds.

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
oekmont - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
             What post cure cycles do you use ?
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
                         Fairing for my bike.
Shaneer22 - 6 Years Ago
                             Just demolded tooling.
Shaneer22 - 6 Years Ago
carbon man - 5 Years Ago
K.C.C - 5 Years Ago
carbon man - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
                             I am out at present will let you no when I get home interesting results.
Shaneer22 - 6 Years Ago
Shaneer22 - 6 Years Ago
                                 + x [quote] [b] Shaneer22 - 12/30/2019 3:56:48 PM [/b] + x [quote] [b]...
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
             Your using x preg.
Shaneer22 - 6 Years Ago
K.C.C - 6 Years Ago
K.C.C - 6 Years Ago
Shaneer22 - 6 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
Warren (Staff) - 5 Years Ago
K.C.C - 5 Years Ago
Warren (Staff) - 5 Years Ago
kip - 5 Years Ago
Warren (Staff) - 5 Years Ago
kip - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
                 Maybe
benji82 - 5 Years Ago
                     I make these ones
K.C.C - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
     some moulds
K.C.C - 5 Years Ago
benji82 - 5 Years Ago
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
             Can you send a pic pls :D
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
K.C.C - 5 Years Ago
Warren (Staff) - 5 Years Ago
K.C.C - 5 Years Ago
Dentex - 5 Years Ago
             It just looks good thats why :D
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
Hanaldo - 5 Years Ago
                 ok thnx
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
Hanaldo - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
K.C.C - 5 Years Ago
SleepingAwake - 5 Years Ago
Hanaldo - 5 Years Ago
Hanaldo - 5 Years Ago
K.C.C - 5 Years Ago
K.C.C - 5 Years Ago
Hanaldo - 5 Years Ago
K.C.C - 5 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search