I'm convinced, the flat cored plate has not enough torque rigidity. The fixing flange is the critical point where the leverage effect it the highest. I would suggest something like a foam cored pan with lattice bracing system on the bottom...just laminated waffle...
That's the high rigidity system.

Rosta Spicl
Rosta Spicl
Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)
Group: Forum Members
Posts: 54, Visits: 250
Sorry, I tought you would like the original U profiles support system put out and replace by laminated structure all around, but it seems not possible - welded to hull. If the panel is fixed on the top of this structure, flat cored panel is OK. But remember, the lattice bracing is more rigid...but heavier of course...

Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
Rosta Spicl - 9/9/2020 11:28:54 AM
Sorry, I tought you would like the original U profiles support system put out and replace by laminated structure all around, but it seems not possible - welded to hull. If the panel is fixed on the top of this structure, flat cored panel is OK. But remember, the lattice bracing is more rigid...but heavier of course...

Hi Rosta Spici, what do you mean by lattice bracing?
Sorry, I don't understand 

Rosta Spicl
Rosta Spicl
Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)Supreme Being (818 reputation)
Group: Forum Members
Posts: 54, Visits: 250
See the waffle. That's generally a pan, supported by lattice structure from the bottom side - it means bottom area of pan filled by crossing ribs fixed to the side flanges of pan. Understand?
Remember, from the rigidity point of view the height of ribs is the much more important than rib width.

Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
Rosta Spicl - 9/9/2020 11:52:45 AM
See the waffle. That's generally a pan, supported by lattice structure from the bottom side - it means bottom area of pan filled by crossing ribs fixed to the side flanges of pan. Understand?
Remember, from the rigidity point of view the height of ribs is the much more important than rib width.

Thank you, understand!
You got me hungry too :-)


Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
Massimiliano - 9/9/2020 12:01:26 PM
Rosta Spicl - 9/9/2020 11:52:45 AM
See the waffle. That's generally a pan, supported by lattice structure from the bottom side - it means bottom area of pan filled by crossing ribs fixed to the side flanges of pan. Understand?
Remember, from the rigidity point of view the height of ribs is the much more important than rib width.

Thank you, understand!
You got me hungry too :-)


Can anyone recommend number of layers and carbon fiber type(s) to achieve the 2mm thickness?

DD-Compound
DD-Compound
Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)
Group: Forum Members
Posts: 25, Visits: 1.1K
You can say roughly 1000g/m2 per mm. We mostly use a 1000g quadraxial two layers each side. That is a laminate that suits to a lot of scenarios.
If you can’t get that use maybe 4 layers of 600g Biax (yes that would be little thicker and heavier but it’s a boat not a airplane)
It is important to make it 0/90/+-45 to get a quasi isotroph laminate.
Also take care on symmetry, otherwise your platform can be twisted badly.
For the core you can bond 2x10mm together but take care it’s bonded proper, otherwise it will delaminate at neutral axis and you will loose stiffness and make sure the holes are not closed, otherwise your infusion will fail.
At that swim Plattform I would go thicker that 20mm and would not put a waffle at the bottom. Then better go to 50mm thickness for stiffness and you are safe. For twist you can add some UD layers but I don’t think that’s needed.

http://www.talkcomposites.com/Uploads/Images/f1d078f0-feab-4db2-8f2f-f009.png
Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
DD-Compound - 9/12/2020 5:52:09 AM
You can say roughly 1000g/m2 per mm. We mostly use a 1000g quadraxial two layers each side. That is a laminate that suits to a lot of scenarios.If you can’t get that use maybe 4 layers of 600g Biax (yes that would be little thicker and heavier but it’s a boat not a airplane)It is important to make it 0/90/+-45 to get a quasi isotroph laminate.Also take care on symmetry, otherwise your platform can be twisted badly. For the core you can bond 2x10mm together but take care it’s bonded proper, otherwise it will delaminate at neutral axis and you will loose stiffness and make sure the holes are not closed, otherwise your infusion will fail.At that swim Plattform I would go thicker that 20mm and would not put a waffle at the bottom. Then better go to 50mm thickness for stiffness and you are safe. For twist you can add some UD layers but I don’t think that’s needed.

Thank you DD-Compound!
I am not able to source any quadriaxal carbon from my suppliers, can a biaxial +/-45° alternated with a twill do the same job?

Hanaldo
Hanaldo
Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Massimiliano - 9/12/2020 6:47:08 AM
DD-Compound - 9/12/2020 5:52:09 AM
You can say roughly 1000g/m2 per mm. We mostly use a 1000g quadraxial two layers each side. That is a laminate that suits to a lot of scenarios.If you can’t get that use maybe 4 layers of 600g Biax (yes that would be little thicker and heavier but it’s a boat not a airplane)It is important to make it 0/90/+-45 to get a quasi isotroph laminate.Also take care on symmetry, otherwise your platform can be twisted badly. For the core you can bond 2x10mm together but take care it’s bonded proper, otherwise it will delaminate at neutral axis and you will loose stiffness and make sure the holes are not closed, otherwise your infusion will fail.At that swim Plattform I would go thicker that 20mm and would not put a waffle at the bottom. Then better go to 50mm thickness for stiffness and you are safe. For twist you can add some UD layers but I don’t think that’s needed.

Thank you DD-Compound!
I am not able to source any quadriaxal carbon from my suppliers, can a biaxial +/-45° alternated with a twill do the same job?

Quadraxials are essentially just 2 layers of biaxials stitched together with one layer flipped over for balance. So yes, it would do the same job - a quad would just save you the effort.

DD-Compound
DD-Compound
Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)Supreme Being (338 reputation)
Group: Forum Members
Posts: 25, Visits: 1.1K
Yes, that will do the same job. A good help is also the R&G or Saertex Material calculator for weights/resin and thickness

http://www.talkcomposites.com/Uploads/Images/f1d078f0-feab-4db2-8f2f-f009.png
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...