Group: Forum Members
Posts: 2.5K,
Visits: 28K
|
I've got a digital gauge, but haven't used it in years. I still find the quickest and most reliable leak indicator is the tone of the pump - I know if my bag is sealed well before my gauge ever settles on a number. That said, mine is not a Greisinger GDH and I understand these are very good, so perhaps mine just isn't as useful as yours.
I do every now and then leave a part under vacuum for days before infusing it, sometimes because I'm waiting for warmer weather, sometimes I just get distracted with other work. Generally, a slight leak will still be present. After 2-3 days, when you reconnect the part to the pump, you will probably hear a slight change of tone for a brief second as that air is evacuated again. If you tug on the bag, it should take 4-5 days to notice any slacking of the bag. This degree of leak is fine, and won't make a difference to the infusion.
|