traces of PVA on the part is fine, it just washes off. The raised parts look like classic bridging where the fabric has not been pressed fully into the corners thus leaving a void. Sometimes this fills with resin, otherwise it stays as an air void which looks a lot worse. You need to take more care with placing the fabric into the mould to ensure there is no bridging.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|