Group: Moderators
Posts: 226,
Visits: 334
|
These calculations do not work out for me, ive tried the calcs with 700grm for mesh etc and never use anything like the amount of resin the formula as says.
just done two panels at 0.5 mtr each with three layers of 200grm cloth, peel ply, mesh, spiral and 600mm of 6mm pipe and used 310grm of IN2 resin per panel.