Group: Forum Members
Posts: 592,
Visits: 1.9K
|
Hi,
I did a few Carbon rings a while back ..
I made a very slightly tapering mandrel from aluminium, and made the rings by laying up narrow strips of CF on this.
wet lay with a lot of resin .. then wrapped in Peelply and shrink tape - Really just a quick & dirty approach ..
When cured i left the rings on the mandrel, removed the tape and peelply and sprayed on several coats of clear coat and chucked the lot back in my lathe and worked on the outside of the rings there. (Sanding and polishing) most of the rings stayed fixed to the mandrel for most of this work ..
I cooled the mandrel in ice-water and then I could knock the rest of them off -- Then finish edges and inside ..
I used several types of CF for the outer layers, the normal twill does not make much of a pattern on a narrow ring, but the EC 90Gsm plain weave looks quite nice.
"Sapere Aude"... Dare to KNOW!
The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...
103% of all people do not understand statistics...
Do not adjust our mind, theres a fault in reality :-)
|