Hy




I have a problem, which i do not know how to solve. For my application i need a thin sheet of carbon fiber that is perfect finish on both sides.




I am using one layer of deltapreg 200g prepreg and vacuumed between two glass panells and than baked in autoclau on 4bar. The problem is no matter what i try i get pinholes on both sides, which are not acceptable. I have also tried with drg carbon with resin and the result is similar.




What can i do to get rid of the pinholes on both sides and get a perfect finish?



Replies
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
There could be many issues causing problems.  Without having experience of your specific pre-preg, as its not one of our products, I can only give general advice.

You might be squeezing out too much resin so perhaps adjust the pressure slightly.  Also consider your gel and flow temperatures of your pre-preg.  You may need to allow it to dwell for a while so the resin can fully flow. 

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
peter_lisica
peter_lisica
Forum Member (43 reputation)Forum Member (43 reputation)Forum Member (43 reputation)Forum Member (43 reputation)Forum Member (43 reputation)Forum Member (43 reputation)Forum Member (43 reputation)Forum Member (43 reputation)Forum Member (43 reputation)
Group: Forum Members
Posts: 5, Visits: 67
Hy the carbon fiber si twill 200g/m2, and the technical data sheet of the epoxy is here http://www.delta-tech.it/pdf/STE%20DT120-6.pdf




What i found is that nearer the edges there are less and less pinholes, to about 2cm from the edge there are no pinholes left.

The main focus is that we get rid of this pinholes on both sides and is not important structuraly.




And another thing that i found out is when i put the glass panel on just one side, the surface was perfect and pinhole free.

How would you recomend the autoclau cycle (pressure and temperatures) to give the best chance of getting what i want.

And also i am wondering what is causing the pinholes. Is it gas forming in the epoxy that can't escape, or is it epoxy bleeding out.




F1rob




Yes the carbon fiber sheet is the same size as the glass panels but i didn't flash tape around so I Will try that also, if the problem is resin bleed.




Regards
Attachments
20150614_164517.jpg (964 views, 3.00 MB)
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
peter_lisica - 10 Years Ago
Warren (Staff) - 10 Years Ago
peter_lisica - 10 Years Ago
f1rob - 10 Years Ago
f1rob - 10 Years Ago
peter_lisica - 10 Years Ago
peter_lisica - 10 Years Ago
Hanaldo - 10 Years Ago
peter_lisica - 10 Years Ago
ChrisR - 10 Years Ago
morepower - 10 Years Ago
scottracing - 10 Years Ago
f1rob - 10 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search