Post Curing Uni-Mould System


Author
Message
ECV3
ECV3
Supreme Being (244 reputation)Supreme Being (244 reputation)Supreme Being (244 reputation)Supreme Being (244 reputation)Supreme Being (244 reputation)Supreme Being (244 reputation)Supreme Being (244 reputation)Supreme Being (244 reputation)Supreme Being (244 reputation)
Group: Forum Members
Posts: 30, Visits: 106
Can anyone give me advice on post curing uni-mould system moulds for use with low to mid temp pre preg. On EC's pdf it says-

10hrs at 60c >  2hrs at 70c >  2hrs at 80c >  2hrs at 90c

My question is are times and temps correct and do i need to use specific Ramp Rates?

Cheers!
Edited 10 Years Ago by ECV3
Reply
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
The temperatures and times are correct.

THe temperature change at each step is relatively small so ramp rates make little difference. The initial upto 60C section most ovens standard rates of around 2C a minute or so will be fine.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search