Hi guys, I'm a furniture designer and after doing a few infusions (and then doing a great 3 day course @ easy composites) I'm absolutely hooked on composites. The possibilities in my field are endless and are barely being touched upon.

I'm currently working on a chair design which is a continuous curve and is usable in two different seating positions (reclined and social). The pattern (plug?) is made and all polished up ready for an infusion and I have an exact 1:6 scale replica for which I've been using to create the test models. I'm having issues with achieving a decent surface quality on the outside face.

I should mention that the final finish I am after on the outside face is the textured matt surface that peel ply leaves. This means that sanding isn't an option. The inside face is glossy.

All layers are securely tacked into place with epoxy spray adhesive. 

The first test had the following layers (working from the inside out):

pattern surface > 3 layers of 200gsm 2/2 twill carbon > peel ply > easy flow mesh > vac bag 

This resulted in a thickness of 0.7mm. The inside face was perfect and the outside was a little bumpy.

The second test was closer to the final desired thickness of 5mm and had the following players (from inside out again)

pattern surface > 1 x 200gsm 2/2 carbon > 1 x 650 gsm 2/2 carbon > 1 x 2mm lantor soric > 2 x 200gsm 2/2 carbon > peel ply (for finish effect) > vac bag

This resulted in a thickness of 3.5mm. The inside face was again perfect but the outside had a very undulated finish with light bunching. The infusion spiral and connectors left deep marks but on the actual pattern this won't be a problem as I have included wide flanges and they will be placed to the sides. This finish isn't even good enough for sanding and then skinning over with a light weave...

I can replace the Lantor Soric with a few layers of 650gms carbon which should give me a slightly better finish I guess... But this would reintroduce infusion mesh and would leave different marks.

So my question is how can I get a nice level and flat peel ply finish on the outside face? I'm pretty much up for trying anything at this point! If this isn't at all possible, what other options do I have? (an outside gloss face wouldn't be durable enough for a chair).

Any help would be extremely appreciated as I'm tearing my hair out at the moment!

Reply
wozza
wozza
Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
No apologies needed its all part of the learning curveSmile not an easy part for your first go. Soric will generally have a slower infusion rate than flow mesh. This can be a good thing, allowing the cloth to fully wet out eliminating pin holes.
The key is getting the resin front to travel evenly across the laminate. That way the resin should reach the vac outlet without leaving some parts lagging behind. If this happens you can end up leaving the feed line open whilst it catches up, result being a resin heavy laminate.
Ideally you want to be clamping off the vac line as soon as it starts to travel up the hose 50mm or so. Leave the feed line open a further 10-20 seconds depending upon the size of the part.
How/wear did you place the spiral, inlet and vac connectors? You may find you need multiple feeds and vac points to get an even infusion.
When not using flow mesh it is possible to get parts of the bag that are not under full vac, the bag can lock itself off if that makes sense.

Warren

Carbon Copies Ltd
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
deagrateful - 12 Years Ago
FLD - 12 Years Ago
ChrisR - 12 Years Ago
wozza - 12 Years Ago
deagrateful - 12 Years Ago
wozza - 12 Years Ago
deagrateful - 12 Years Ago
Hanaldo - 12 Years Ago
wozza - 12 Years Ago
deagrateful - 12 Years Ago
wozza - 12 Years Ago
wozza - 12 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search