Female canoe mold difficulies


Author
Message
Zedok
Zedok
Supreme Being (122 reputation)Supreme Being (122 reputation)Supreme Being (122 reputation)Supreme Being (122 reputation)Supreme Being (122 reputation)Supreme Being (122 reputation)Supreme Being (122 reputation)Supreme Being (122 reputation)Supreme Being (122 reputation)
Group: Forum Members
Posts: 18, Visits: 115

Good afternoon to all,

I am building a female mold that will beused to make a carbon fibre marathon canoe (18’6”). I have good skills working with fibreglass but this is my first experience in making a femalemold.

The mold is based on wooden slats lined with 1” foam and  lined once more with fibreglass. The fibreglass  is then finished with the usual body fillerand mold primer/hi-gloss coats to make it a glass finish. As you may realise,the front and back end of the molds are extremely streamlined and I find itimpossible to sand down to a glass finish.

The alternatives that I have come up withwould be to 1) cut the mold in half and work on each side separately thenreassemble to lay the carbon fibre cloth. The disadvantage might be that Iwould not end up with symmetrical sides. Option 2 would be to lay the carbon fibrein the mold as is but finish the exterior of the canoe’s ends to a glass finishafterwards. Finishing the outside to a glass finish after unmolding seemsdifficult to achieve. Any comment and recommendation would be welcome. 

Manythanks.


Z


Reply
Dravis
Dravis
Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
Hi again...

From looking at the picture I can already see that you can not make that shape in a non split mold... there are at least two places on both sides where you have the shape going inwards towards the top edge. that will lock the body of the canoe into a single piece mold... even IF you can press the sides together enough to clear the top of the mold, you will have a lot of problems de-molding...

Even if you modify the shape to avoid the inward slopes on the top of the canoe, the very narrow places at either end will be very difficult to release, since you will also have great difficulty in polishing it in the very confined spaces in the bottom "corners" They WILL stick or lock solid ...

I certainly would much rather do this as a split mold, and avoid several problems at once.
You will have another problem with the split mold, you will have a slight edge along the seam of the split mold, but if you make sure that there is room for a bit of extra Gel-coat along the seam, that can be polished away.

I would definitely go for a clear gelcoat in the mold first.  Are you going to use Polyester?

@george:  I do not think the canoe in the picture is the actual one... it is what he is aiming to build, not having one to use as a "plug" to build a mold over, he is building the mold as a female mold, to use directly.. in effect "sculpting" the canoe "inside out" .. or should that be "outside in" Rolleyes

I have made a "plug mold" the same way, for the inside shell of a custom motorcycle seat.   since the underside of the seat shell is going to be the visible side, I decided to jump one step and laminate the seat shell directly over a reusable "plug"  made from MDF and coated with a thick layer of tooling epoxy resin with filler followed by a layer with only a bit of graphite powder and then polished and waxed ...  The "plug mold is looking great, but I haven't had time to try it yet..  BigGrin

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Zedok - 12 Years Ago
Dravis - 12 Years Ago
Zedok - 12 Years Ago
George Sychrovsky - 12 Years Ago
Dravis - 12 Years Ago
Zedok - 12 Years Ago
George Sychrovsky - 12 Years Ago
Dravis - 12 Years Ago
Zedok - 12 Years Ago
wozza - 12 Years Ago
Dravis - 12 Years Ago
Zedok - 11 Years Ago
     Looking good :)
Dravis - 11 Years Ago
Zedok - 11 Years Ago
Hanaldo - 11 Years Ago
Dravis - 11 Years Ago
Zedok - 11 Years Ago
Hanaldo - 11 Years Ago
VVS - 11 Years Ago
Dravis - 11 Years Ago
Zedok - 11 Years Ago
Zedok - 11 Years Ago
Zedok - 11 Years Ago
Zedok - 11 Years Ago
VVS - 11 Years Ago
Zedok - 11 Years Ago
Zedok - 11 Years Ago
Dravis - 11 Years Ago
Zedok - 11 Years Ago
Dravis - 11 Years Ago
Zedok - 11 Years Ago
Hanaldo - 11 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search