Hello everybody,

I got very helpful answers from you guys last time, so I decided to ask again Wink

In my infusion process I use low viscosity infusion resin. When I try to degas it with my home-made chamber I get many bubbles escaping from my pot and forming a big foam on the surface. This is endless Wink
I use full power of my vacuum pump (nearly -1.0). I've never managed to get clear liquid after degassing.

What should I do to improve it and make it more effective?

Sorry for my english,

Thanks!

Peter/Poland
ChrisR
ChrisR
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 363, Visits: 3K
is it an epoxy infusion resin?
_pepis
_pepis
Forum Member (27 reputation)Forum Member (27 reputation)Forum Member (27 reputation)Forum Member (27 reputation)Forum Member (27 reputation)Forum Member (27 reputation)Forum Member (27 reputation)Forum Member (27 reputation)Forum Member (27 reputation)
Group: Awaiting Activation
Posts: 5, Visits: 47
Yes. Epoxy resin for infusion.

Peter
20_rc51_00
20_rc51_00
Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)
Group: Forum Members
Posts: 95, Visits: 548
how long do you let it degass for? Hoe much volume resin are you degassing? Are you using a tall narrow cup or a wide cup of resin?
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
Here are some tricks that might help:

- heat your A+B before mixing to lower the viscosity, then mix and degass
- Use a mixingcup/pot with a large bottom surface
- Try using a vent between the pump and the chamber, to be able not to pull full vacuum all the time.
  If you pull 80% vacuum in the begining, it will degass without rising, then add more vacuum till perfect 

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




fiberpro
fiberpro
Supreme Being (89 reputation)Supreme Being (89 reputation)Supreme Being (89 reputation)Supreme Being (89 reputation)Supreme Being (89 reputation)Supreme Being (89 reputation)Supreme Being (89 reputation)Supreme Being (89 reputation)Supreme Being (89 reputation)
Group: Forum Members
Posts: 13, Visits: 70
I heard from technicans that it is possible to self degass resin just while infusing, have you guys tried?