Anyone have experience with TenCate OOA's ?


Author
Message
20_rc51_00
20_rc51_00
Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)
Group: Forum Members
Posts: 95, Visits: 548
http://www.ambercomposites.com/prepreg/out-of-autoclave-prepreg/

anyone have any experience with this?

I live in Canada and I'm having a hard time tracking down any OOA materials. Anyone have suggestions for anything in Canada or the USA? Alternatively I might have to bit the bullet and buy from somewhere in Europe....

Any other sources would be appreciated. 

Until now I've been doing infusions but I'm really tired of the whole infusion process and need a change. Its a PITA with the whole layup and then the trimming afterward. Prepreg might just let me cut back on the amount of post production trimming....
Replies
20_rc51_00
20_rc51_00
Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)
Group: Forum Members
Posts: 95, Visits: 548
One more question since I have not worked with prepregs,

What level of "tack" is preferable? I'm would assume it is somewhat dependent of the intricacies of the tool but would you give some idea of a good handling level of tack? Is too much problematic is too little lead to distorition/movement of the stack?
THanks
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
for me the ooa of easy composites is perfect, nice tack on the surface of the mould...by having it that way it wont lift when adding the layers on top of that...did some test with a prepreg with less tack and I got annoyed while working with it, each time I've added a layer and tried to press it down, it got away from the surface of the mould

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




20_rc51_00
20_rc51_00
Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)
Group: Forum Members
Posts: 95, Visits: 548
THanks, I would assume that too high of tack might reduce the drapability/adaptability into very tight areas if the rest of the reinforcement is already laid down into the mold....too little tack and you aren't sticking to the mold just like you mentioned. 
ChrisR
ChrisR
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 363, Visits: 3K
List of some prepreg companies supplying USA
http://www.compositesworld.com/suppliers/product/294

Gurit USA may be of help, it depends how much you need as most prepreg suppliers have a MOQ of 10 or 20m/yrds but also the problem with sourcing from the UK if you go that way is the uncontrolled temperature during transport and duration, if you have a prepreg with an outlife of 7 days and it takes 5/6 days to get there then there is little usable life in it.

Amber composites are pretty good, played with a few but usually subject to minimum order quantities, sometimes you can get 2nds quality but "ya pays ya money and takes ya chance" sometimes its just a few inclusions or weave distorsion every so often but other times the whole thing is pretty much junk.

When you use prepreg then consolidation/debaulking can make the process more labourious than infusion.

You don't always have to use an OOA prepreg, a lot of the time the lower temperature ones such as ambers 8020 and E644/650 are very usable vacuum only.

You will also find voids and bridging more common especially on more complex moulds as there isn't the spare resin to fill them, if you don't force each layer into every nook and cranny then you will have more problems.
20_rc51_00
20_rc51_00
Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)Supreme Being (683 reputation)
Group: Forum Members
Posts: 95, Visits: 548
Thanks Chris, appreciate the link and tips.

I need a change from infusion, the thought of it is daunting to me. And I dread the trimming of mass excess material (because laying fabric perfectly matched in size is just asking for trouble imo). I also get anxiety attacks  Blink about the reinforcement stack shifting during handling or loose fibers on the cosmetic side etc etc... I'm pretty obsessive about bridging, I wouldn't foresee that as a stumbling block for me. 

regarding the debulking, this is to reduce entrapped air (as much as can be before resin flow/viscosity reduction with heat anyways) and reinforcement consolidation right? How long typically for debulking? when do you know that it's "enough"/ what is the observed end goal?

ChrisR
ChrisR
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 363, Visits: 3K
20_rc51_00 (24/01/2014)
Thanks Chris, appreciate the link and tips.

I need a change from infusion, the thought of it is daunting to me. And I dread the trimming of mass excess material (because laying fabric perfectly matched in size is just asking for trouble imo). I also get anxiety attacks  Blink about the reinforcement stack shifting during handling or loose fibers on the cosmetic side etc etc... I'm pretty obsessive about bridging, I wouldn't foresee that as a stumbling block for me. 

regarding the debulking, this is to reduce entrapped air (as much as can be before resin flow/viscosity reduction with heat anyways) and reinforcement consolidation right? How long typically for debulking? when do you know that it's "enough"/ what is the observed end goal?


If you are paranoid now, wait till you use prepreg! I really like the stuff and enjoy working with it. If you are careful then you can offset some of the additional cost of the stuff as you don't have so much waste if you nest the pattern cut outs propperly.

Depending on the matrix, some require debaulking under vacuum only for x hours/mins (usually on datasheet) and others require an elevated cure during the debaulk, again see the materials datasheet. The idea is that you consolidate the ply's in stages to minimise voids, bridging and thickness change during final cure plus you can control the resin ratio a bit more closely by bleeding some out if required
morepower
morepower
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 242, Visits: 1.2K
matthieutje65 (23/01/2014)
for me the ooa of easy composites is perfect, nice tack on the surface of the mould...by having it that way it wont lift when adding the layers on top of that...did some test with a prepreg with less tack and I got annoyed while working with it, each time I've added a layer and tried to press it down, it got away from the surface of the mould

The problem is that is is expensive.... especially for someone in the USA... If there is a Cytec distibutor willing to do smaller quantity minimum orders then it is better if he can do that.. It is the best material but the cost from either easy composites or cytec are now not worth the extra cost if you look at how much it can cost to coat a part especially a large part.. If I used £1000 worth of VTF/Easy Preg or £350 worth of another material which is close on finish that leaves a lot of spare cash to pay to have it sprayed... I have had a full motorcycle kit lacquered for £150.00 making a total cost minus consumables and oven time of £500. It is simple math.... 

I would use VTF for everything if I could afford it... I cant and I have never paid more than £68.00 inc VAT for VTF but now they have upped the minimum quantity I have had to look else where.. I now pay just over £30 per meter and get great results which is more profitable for me.... I can also get plain weave which I cannot get in the VTF/easy preg materials..

If I can get finishes like this out of the mould... I would do what the OP is doing and shop round and find a material an learn how to make it work for them...


A set of these if I only used easy preg would have cost me almost £100 to make in materials and power.. Using the material I now use they cost me £35 to make. 
Edited 11 Years Ago by morepower
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
20_rc51_00 - 11 Years Ago
matthieutje65 - 11 Years Ago
20_rc51_00 - 11 Years Ago
morepower - 11 Years Ago
20_rc51_00 - 11 Years Ago
20_rc51_00 - 11 Years Ago
matthieutje65 - 11 Years Ago
20_rc51_00 - 11 Years Ago
ChrisR - 11 Years Ago
20_rc51_00 - 11 Years Ago
ChrisR - 11 Years Ago
morepower - 11 Years Ago
fgayford - 11 Years Ago
20_rc51_00 - 11 Years Ago
morepower - 11 Years Ago
20_rc51_00 - 11 Years Ago
morepower - 11 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search