https://fbcdn-sphotos-e-a.akamaihd.net/hphotos-ak-prn2/1397594_10151780075843045_672071466_o.jpg

I have attempted to cast a model using Easy Composites' Fast Cast Polyurethane Casting Resin. The cast failed as the resin did not fully cure. Half the model cured but the rest came out like thick honey, see image above. I'm not sure why this happened, but my immediate problem is, how do I clean the uncured resin goo from my mold? The mold is made of RTV silicone.

Edited 12 Years Ago by moif
Replies
moif
moif
Forum Member (48 reputation)Forum Member (48 reputation)Forum Member (48 reputation)Forum Member (48 reputation)Forum Member (48 reputation)Forum Member (48 reputation)Forum Member (48 reputation)Forum Member (48 reputation)Forum Member (48 reputation)
Group: Forum Members
Posts: 4, Visits: 49
I mixed 170 grammes in total. I don't know if thats a big mix or not, as these are my first attempts at resin casting
Zorongo
Zorongo
Supreme Being (276 reputation)Supreme Being (276 reputation)Supreme Being (276 reputation)Supreme Being (276 reputation)Supreme Being (276 reputation)Supreme Being (276 reputation)Supreme Being (276 reputation)Supreme Being (276 reputation)Supreme Being (276 reputation)
Group: Forum Members
Posts: 40, Visits: 330
You have to be very carefull when mixing small quantities.

If you mix 85 + 85 gr from two diferent cups you may (:pinchSmile have a problem. 
 
When you stir B component into A, you have to asure to drain EVERY GRAM.

I mean: If 5 grams from B stay on the cup's wall, it represent about a 6% of the B component. You will be mixing 85 gr A + 80 gr B.

This % of lost material is bigger as the mix is smaller.

What you can do to avoid that, is to mix on the same cup.

Stir the A 85 grams first. Then, on the same cup, add another 85 gr B. Then mix everything carefully.

(always mix each component separately before mixing)
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search