Advanced guide - Working with pre-pregs


Author
Message
mawgan
mawgan
Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)Supreme Being (104 reputation)
Group: Forum Members
Posts: 12, Visits: 32
I am new here and have had a quick look through the forums and on the easy composites website/videos and I have yet to see any real advanced techniques shown (please correct me if I'm wrong and there is in fact advanced tutorials somewhere that state the techniques that I am referring to).

I have personally had over 10 years experience working with all aspects of advanced composites and the family run company that I own has been in the business for over 30 years. We have worked mostly in marine but have covered all aspects along the way from F1 through to aerospace.

I thought that I would list just a few things here and people can maybe carry this on and extend any knowledge/tips they may have learnt along the way.

To start with, no matter what composite project you are working on, it is all in the preparation, it is the most important thing. I.e, cutting materials correctly and all consumables ready to go before you even think about getting started. Working cleanly is also very important and something you learn working professionally within the industry. I will post some of my top tips of preparation and working cleanly later on this thread.

For now a couple of advanced pre-preg tips:

Spike rollers - I have not seen these listed anywhere on this forum or the main site, if you do not know what I refer to, it is basically a roller with spikes sticking out. It is important to spike roller each layer of pre-preg that you put down in the stack as this creates small holes within the otherwise solid resin structure for any air pockets to escape during debulking.

Debulking - As a general rule of thumb you should always debunk every 2 layers, along with the spike roller this gets rid of air pockets trapped in the stack and helps 'set' the pre-preg in place as you go.

Breather tows - A breather toe is simple a short tow of fibreglass placed around the edge of the laminate (in the area to be trimmed), you should place one tow roughly every 250-500mm for large panels/mouldings and smaller distances apply for smaller jobs. This is more important with infusion and Sprint system pre-pregs as it enables the air to escape more easily between layers but also applies to pre-preg as well if you want to do a professional job.

Pre-preg curing - I have had a quick look through the easy composites pre-preg offering and was surprised to find fairly basic information regarding the resin systems used and the cure process. Not anywhere mentioned is the recommended ramp rate for cure which is extremely important. As a general rule of thumb anywhere from 0.3C to 2C per minute is acceptable but this really depends on the application and should be specified by the manufacturer. Ramp rates allow the resin to flow correctly eliminating pin holes and voids and it allows the cured resins tg1 to stay ahead of the 'cure'.

Dwell times - A dwell is a temperature hold for a set period of time in order for the stack and mould to catch up with the rest of the cure, this all depends on the oven and should be analysed using oven test before curing any pre-preg. Once you have learnt your oven you can apply this to all future cures and can set an appropriate dwell time.

That concludes just a few things that I have noticed were never mentioned thus far. I am working on a very detailed pre-preg guide which will include many tips and goes into extreme detail in order to achieve results seen in the most advanced racing yachts/f1/aerospace applications. Please let me know if you are interested in this.

Please feel free to add any other advanced suggestions on working with pre-pregs and I will post more up when I have time.

Thanks and I hope this helps anyone interested.
Replies
morepower
morepower
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 242, Visits: 1.2K
Warren (Staff) (22/08/2013)
Its horses for courses at the end of the day.

Sure no ones doubting that pre-preg parts are the pinnacle of the industry at the moment.

But twice the material cost for something thats maybe 20% stronger and lighter.

Clearly not worth it for most people for larger panels.  But it does have its place for smaller, complicated parts where material cost isnt such an issue.


Twice the cost?? Dry cloth is about £20 per sq/m and resin works out about another £5 per sq/m  Plus you need pipes and other consumables spiral tube and infusion mesh which is just under £6 per meter and there will be some extra resin wastage in the pipes through to the catch tank. So that is up to about £31 per sq/m plus VAT.

Pre-preg can be had for between £36 and £48 per sq/m depending on which material you have and the PRF material is good enough for most people at less than £40 per sq/m.

 

This is using a pre-preg that cost less than £40.00 per Sq/m and a motorcycle body kit is anything but small... But I have a week to lay up the parts and can take my time getting it all done.



The equipment when laying up is no different to wet lay vac bagging so you can do both for no extra cost... My "oven" cost me £27 for the PID, Solid state relay and sealed electrical box, thermocouple and a £40 3kw fan heater... I can either use simple card board boxes for small parts or a clean garden wheelie bin for larger parts then if you have space you can use Kingspan insulation to make a large oven and only need to get a better fan and some ducting. That would cost about £400 to build and you can still use the heater and controller ect with any oven you build of varying size if you want as it will work with any box. One other thing I would use, but many dont, a remote wireless display meat thermometer to just check the temp of the actual part too...

So the set up is a little more than setting up for infusion but there are less ongoing consumables needed and you have parts that are 20% lighter and stronger. The cost of materials is possibly 25% more expensive but when you look at the value of those parts if you are going to sell them many would rather have simple wet lay for cheapness or if they want the real deal only pre-preg is going to get the highest prices. 
carboncactus
carboncactus
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 243, Visits: 1K
morepower (22/08/2013)




I like that carbon kevlar chain guard / side panel

http://www.talkcomposites.com/Uploads/Images/db628ad5-e0e7-47b9-873a-3d84.png
morepower
morepower
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 242, Visits: 1.2K
carboncactus (23/08/2013)

I like that carbon kevlar chain guard / side panel


Cheers.... I did some to see what people think.... Not to popular to be honest... I like them a lot.... But people are wrapped up in wanting carbon.... lol.
andygtt
andygtt
Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)
Group: Forum Members
Posts: 157, Visits: 1.2K
morepower (22/08/2013)
Warren (Staff) (22/08/2013)
Its horses for courses at the end of the day.

Sure no ones doubting that pre-preg parts are the pinnacle of the industry at the moment.

But twice the material cost for something thats maybe 20% stronger and lighter.

Clearly not worth it for most people for larger panels.  But it does have its place for smaller, complicated parts where material cost isnt such an issue.


Twice the cost?? Dry cloth is about £20 per sq/m and resin works out about another £5 per sq/m  Plus you need pipes and other consumables spiral tube and infusion mesh which is just under £6 per meter and there will be some extra resin wastage in the pipes through to the catch tank. So that is up to about £31 per sq/m plus VAT.

Pre-preg can be had for between £36 and £48 per sq/m depending on which material you have and the PRF material is good enough for most people at less than £40 per sq/m.

This is using a pre-preg that cost less than £40.00 per Sq/m and a motorcycle body kit is anything but small... But I have a week to lay up the parts and can take my time getting it all done.


no way I use £5 of resin per square meter of cloth... and I only use the same amount of infusion mesh etc regardless of layers... so a 4sq meter layup with 4 layers of carbon/kevlar using resin infusion is around £420 all consumables and resin.

For pre preg thats over £680 (guessing £40 consumables tape, bag, breather etc)

Im going to give pre preg a go at some stage, but for a DIY making body panels I see the cost of storing the materials long term as very high indeed... Id also need a massive oven (could do with one now tbh but it isnt a must have yet).

One thing I would like to know... the difference in strength is mainly the resin properties... how strong/weak is the resin infusion resin compared to pre preg?
morepower
morepower
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 242, Visits: 1.2K
I got an 8 foot commercial freezer for £230.00 lol... Making an oven is not hard but it does take up space and the bigger the part the more space. I am lucky I can convert an old outside toilet into an oven. So I have 7 feet deep 4 feet wide and 9 feet high if I want to use it all.. So I still have all my workshop space and not have an oven taking up space.. So I am lucky... But the costs if you look round are not that high compared to many other manufacturing businesses like engineering ect... 

You may find you can lose a layer of material or two in places and only add pre-preg where it is needed to get the strength where you need it.... My seat unit is 2 layers thick where it has no structural requirement but 10 to 15 layers thick where I need a lot of strength... It just depends where you need to have strength or just need something to create the shape.... lol
Edited 12 Years Ago by morepower
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
mawgan - 12 Years Ago
wozza - 12 Years Ago
mawgan - 12 Years Ago
wozza - 12 Years Ago
mawgan - 12 Years Ago
compositepro - 12 Years Ago
andygtt - 12 Years Ago
Shaneer22 - 12 Years Ago
Warren (Staff) - 12 Years Ago
morepower - 12 Years Ago
carboncactus - 12 Years Ago
morepower - 12 Years Ago
wozza - 12 Years Ago
compositepro - 12 Years Ago
Warren (Staff) - 12 Years Ago
morepower - 12 Years Ago
                 [quote][b]morepower (22/08/2013)[/b][hr]...
carboncactus - 12 Years Ago
morepower - 12 Years Ago
andygtt - 12 Years Ago
morepower - 12 Years Ago
wozza - 12 Years Ago
morepower - 12 Years Ago
TomDesign - 12 Years Ago
morepower - 12 Years Ago
TomDesign - 12 Years Ago
morepower - 12 Years Ago
morepower - 12 Years Ago
TomDesign - 12 Years Ago
fgayford - 12 Years Ago
mawgan - 12 Years Ago
fgayford - 12 Years Ago
Airship-Jim - 12 Years Ago
Airship-Jim - 12 Years Ago
morepower - 12 Years Ago
TomDesign - 12 Years Ago
morepower - 12 Years Ago
mawgan - 11 Years Ago
FLD - 11 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search