Does easy lease have a shelf life?

I am having all sorts of problems getting your infusion resin to release from your uni-mould product.

I have lost several moulds and plugs now, and can only put it down to the release agent.
I bought the current batch of easy lease from you over a year ago now, does it lose its effectiveness?
Reply
Warren (Staff)
Warren (Staff)
Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Warren is right. The recommended shelf life is 1 year in a sealed container.

If you havent used the lid as much then it will soak up moisture and degrade.

Also if youve been using it in the recent hot weather you will find it evaporates off silly fast at anything near 30C let alone over it. I had a sticker last year in the heat wave and was working around 30C and it was evaporating off as fast as i put it on, so even with what i though was 5 coats it was quite possible to have a few patches that were a bit ropey and enough to stick.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant