Mould ruined after 1st use..


Author
Message
carbon man
carbon man
Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)
Group: Awaiting Activation
Posts: 86, Visits: 1.2K
Hi, this mould is made from high temp epoxy and oven for 17 hours following the data sheet. 

I think I could of took more care in mould prep which didn't help. But it had about 8 coats of easy lease and struggled to out. Now the mould has carbon print through and cracked gel?

Carbon use xpreg xc110 oven cured following standard curing cycle.

Edit : carbon was in the mould over night before going in the oven as it was getting late and could fix leak in the bag.

Edited 5 Years Ago by carbon man
Replies
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
How accurate were you with your mix ratio when you made the mould? It does look/sound like an under-curing issue. I've had similar before and realised I had used the wrong mix ratio. The mould cured hard enough that I didn't notice anything was wrong, but was obviously still very open to bonding.

Could also simply be a release failure as well though. Is that surface finish the finish you wanted on your mould, or did it dull off during the cure? If it dulled during the cure then I would say it's an under curing issue for sure.
carbon man
carbon man
Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)Supreme Being (758 reputation)
Group: Awaiting Activation
Posts: 86, Visits: 1.2K
Hanaldo - 6/28/2020 10:17:13 PM
How accurate were you with your mix ratio when you made the mould? It does look/sound like an under-curing issue. I've had similar before and realised I had used the wrong mix ratio. The mould cured hard enough that I didn't notice anything was wrong, but was obviously still very open to bonding.

Could also simply be a release failure as well though. Is that surface finish the finish you wanted on your mould, or did it dull off during the cure? If it dulled during the cure then I would say it's an under curing issue for sure.

Yeah all ratios weighed out and mixed properly, and yeah the mould was dull I was ok with that because it was getting clear coated. Next time I might make mould glossy to help with release 

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
carbon man - 5 Years Ago
explorecomposites - 5 Years Ago
carbon man - 5 Years Ago
Hanaldo - 5 Years Ago
carbon man - 5 Years Ago
Fasta - 5 Years Ago
             No? Just mould cleaner
carbon man - 5 Years Ago
Fasta - 5 Years Ago
Hanaldo - 5 Years Ago
oekmont - 5 Years Ago
carbon man - 5 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search