Hello, 
I am currently producing an infused complex carbon fiber part with a clear gelcoat CRYSTIC GELCOAT 253PA by Scott Bader. After some testing we concluded that multiple very thin passes need to be applied to avoid the gelcoat from getting cloudy. This being said we have to rely on the gelcoat operators expertise and the part in particular is extremely difficult due to deep cavities. I was thinking about infusing the part without a gelcoat and then applying an automotive clear coat on the part as a solution.

What are your thoughts on this? Any suggestions for an in mould applicable clear gelcoat that would have good cohesion with epoxy and not get cloudy when exposed to the sun?
What does the automotive industry do to avoid this?

Thank you
Replies
Classicarbon
C
Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)
Group: Forum Members
Posts: 86, Visits: 639
Warren (Staff) - 9/10/2019 3:54:36 PM
You can apply some gels by brush but it isn't recommended for infusion.  This is because it is hard to avoid brush marks and when infused, the fabric is pressed on the uneven surface distorting it slightly so you can see some fibre distortion when brushed gel is infused.  Brushed gel is fine for wet lay or vacuum bagging as there is a layer of wet resin between the gel and cloth for the cloth to float on and even things out.  

So if not brush then better to use only clear coat after part is ready?

MarkMK
MarkMK
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 338, Visits: 2K
If you've got the space in which to do it, then investing in a compressor and cup gun would be the easiest DIY solution so that you can use the spray in-mould coating

Failing that, spraying the parts with an auto-quality 2-pack clear coat is another way of having your parts coated. This would most likely entail finding a professional sprayer to complete the job, though, as not a job to tackle in the garage given the additional safety requirements


Edited 6 Years Ago by MarkMK
Classicarbon
C
Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)
Group: Forum Members
Posts: 86, Visits: 639
MarkMK - 9/11/2019 10:45:29 AM
If you've got the space in which to do it, then investing in a compressor and cup gun would be the easiest DIY solution so that you can use the spray in-mould coating

Failing that, spraying the parts with an auto-quality 2-pack clear coat is another way of having your parts coated. This would most likely entail finding a professional sprayer to complete the job, though, as not a job to tackle in the garage given the additional safety requirements


Yeah,you read my mind. I'm begginer so if part come out right will think about next steps. So it's fine to use mould release, wax etc. To be able take the part out?

MarkMK
MarkMK
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 338, Visits: 2K
If you do opt to use something like the GC50 in-mould gel coat, then semi-permanent release agent is all that would need to get reliable releases. As Warren said, application by brush wouldn't work well if processing parts via infusion, as the hardened surface of the coating would end up too uneven to provide a good cosmetic finish




GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
cfrpbhs - 6 Years Ago
Warren (Staff) - 6 Years Ago
             Can the gelcoat be applied with brush?
Classicarbon - 6 Years Ago
MarkMK - 6 Years Ago
Warren (Staff) - 6 Years Ago
Classicarbon - 6 Years Ago
MarkMK - 6 Years Ago
Classicarbon - 6 Years Ago
MarkMK - 6 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search