You can apply some gels by brush but it isn't recommended for infusion. This is because it is hard to avoid brush marks and when infused, the fabric is pressed on the uneven surface distorting it slightly so you can see some fibre distortion when brushed gel is infused. Brushed gel is fine for wet lay or vacuum bagging as there is a layer of wet resin between the gel and cloth for the cloth to float on and even things out.