Whats the chances of a uni mould being porous? 

Im on my second attempt at trying to get a leak free bag on this car hatch back but still no luck.
I feel I'm no amateur at the bagging process but not having much joy with this one.

scottracing
scottracing
Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)
Group: Forum Members
Posts: 460, Visits: 5.2K
Have you done a drop test with a vac gauge? Just bag up the mould without any material and see if theres a vac drop, id it a 1 piece mould or has it several parts /  joins?
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
you have chances to get leaks, 
But I think its all a matter of how you work on your mould...
If you use all the steps; gelcoat, coupling coat, tooling resin (4 layers) the chances are minimal! 
make sure you have no airpockets in your tooling resin coats by using a roller and tighten all the corners firmly against your part while making the mould. 

If you want to be fully sure; I sand the back of the mould once cured, removing all sharp edges and coat it again with a thick layer of resin.

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




Darren
Darren
Supreme Being (406 reputation)Supreme Being (406 reputation)Supreme Being (406 reputation)Supreme Being (406 reputation)Supreme Being (406 reputation)Supreme Being (406 reputation)Supreme Being (406 reputation)Supreme Being (406 reputation)Supreme Being (406 reputation)
Group: Forum Members
Posts: 54, Visits: 916
I decided to bite the bullet and infuse the part.
Found to tiny leaks in the actual bagging film, sealed them off with some bagging tape and all worked out ok.