Hi all,

Im trying the new XC110 prepregs but i seem to get no nice results at all. with other (cheaper) prepregs i get really nice and smooth surfaces.
Here is what the parts look like. The oven was set at the values from the curing data sheet. im using thin mould from tooling gelcoat and epoxy/fiberglass.
The tempsensor was laying on the mould itself. should i try increasing more heat at the soak from 4 hours at 70 degrees?







Hanaldo
Hanaldo
Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Looks like there is a bit of bridging that wont be helping. I would try moving the temperature probe for a start, I've never ever had good results with the probe sitting on the part. 

What tooling gelcoat are you using??
Warren (Staff)
Warren (Staff)
Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Extending the soak time can sometimes help for complex shaped moulds or parts with lots of layers.  Ignoring the bridging which is an issue in its own right, was the tooling gelcoat and mould all fully postcured and suitable for a 120C cure?  How many layers of pre-preg were used?


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Thomb
Thomb
Supreme Being (287 reputation)Supreme Being (287 reputation)Supreme Being (287 reputation)Supreme Being (287 reputation)Supreme Being (287 reputation)Supreme Being (287 reputation)Supreme Being (287 reputation)Supreme Being (287 reputation)Supreme Being (287 reputation)
Group: Forum Members
Posts: 23, Visits: 656
Warren (Staff) - 12/3/2018 10:03:14 AM
Extending the soak time can sometimes help for complex shaped moulds or parts with lots of layers.  Ignoring the bridging which is an issue in its own right, was the tooling gelcoat and mould all fully postcured and suitable for a 120C cure?  How many layers of pre-preg were used?

The mould is used before with other prepregs. The layers i used on this one were 1x210 and 1x420. The previous results were way better.




Edited 8 Years Ago by Thomb
Warren (Staff)
Warren (Staff)
Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
That looks like our EG60 Tooling gelcoat which with a post cure is only rated to 80C at best.  Certainly the 120C section of the cure will be pushing what it is capable of which may explain the matt finish. 


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
cpkielycua
cpkielycua
Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)Supreme Being (339 reputation)
Group: Forum Members
Posts: 29, Visits: 285
What other prepreg do you use?
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search