Good afternoon

I've read all the topics in this forum but I'm still confused so I kindly ask an help.

I’m experimenting the production of a compression mould by using my 3D printer.
The part I want to manufacture is made by Carbon fiber and has 1.2mm thickness. I want to cure it at room temperature at the beginning and if everything is OK I will cure in a oven at 60°C in the future.

Here a picture of my 3D printed mould (made by ABS but I can choose different material  such as PLA, Polycarbonate, ASA and so on).
I have removed all the 3D printing layers and defects by using sand paper; here is how it looks like at the end of the sanding process:


I have applied 7 layers of releasant wax and polysh the mouls after the last one by using a clean cloth.
I have prepared a sandwich of carbon fiber and resin and put inside the compression mold and squeeze it by using 300Kg of weight; I cure it at room temperature.

Here the picture if my first carbon fiber trial part.
Please note that the right side has been painted because the CF part just out of the mould has a matte finish which I don't like at all (I want a gloss finish without any additional painting or polish treatment). I can see major defects which I think are due to a lack of material (my sandwich was too thin) and I'm not worry about it.



How can I get a gloss finish on my carbon fiber part just out of the mould ?
Is it true that the only way to get a gloss carbon fiber part is to have a gloss mould surface? If the answer is yes, can you explain me the reason ?

If I need to treat my 3D mould (ABS material) so it became gloss, which process and materials do I have to purchase?
I’ve read about filler and other stuff but I’m a little bit lost because normally a 3D printed mould is not commonly used.

Can I use S120 directly on the ABS (or PLA, Polycaronate, ect) mould or do I have to apply a primer first?
Or do I have to apply to the mould an epoxy resin first?
I'm a little bit lost and confused because all the info I found are not referred to compression mold and do not require a gloss finish carbon fiber part as I would like.

Thanks in advance for your help.

Edited 7 Years Ago by Matteo Dapporto
Replies
f1rob
f1rob
Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)
Group: Forum Members
Posts: 237, Visits: 4.8K
Use marbocote 2002
Print your mould
Rub the lines out
Apply 6-10 coats of 2002 depending on the porosity of the part (Can oven between coats)
We nib an smooth with 1200 paper
Apply one last very wet coat an let dry naturally
You will have a mirror like Finnish ( thou you can still polish more) that will be good for anything up to 125deg pre preg
For ultimate shine ( and at a lower temp) use a wax release like freewax from freecote
Matteo Dapporto
M
Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)
Group: Forum Members
Posts: 10, Visits: 77
f1rob - 10/11/2018 2:09:44 PM
Use marbocote 2002
Print your mould
Rub the lines out
Apply 6-10 coats of 2002 depending on the porosity of the part (Can oven between coats)
We nib an smooth with 1200 paper
Apply one last very wet coat an let dry naturally
You will have a mirror like Finnish ( thou you can still polish more) that will be good for anything up to 125deg pre preg
For ultimate shine ( and at a lower temp) use a wax release like freewax from freecote

Thanks!
Does 2002 stick to ABS and PLA materials?
Because in the tech spec it's not mentioned.

MAtteo

f1rob
f1rob
Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)
Group: Forum Members
Posts: 237, Visits: 4.8K
Matteo Dapporto - 10/11/2018 2:16:52 PM
f1rob - 10/11/2018 2:09:44 PM
Use marbocote 2002
Print your mould
Rub the lines out
Apply 6-10 coats of 2002 depending on the porosity of the part (Can oven between coats)
We nib an smooth with 1200 paper
Apply one last very wet coat an let dry naturally
You will have a mirror like Finnish ( thou you can still polish more) that will be good for anything up to 125deg pre preg
For ultimate shine ( and at a lower temp) use a wax release like freewax from freecote

Thanks!
Does 2002 stick to ABS and PLA materials?
Because in the tech spec it's not mentioned.

MAtteo

Well so far it's worked on every single bit we have done but we make parts for lots of different teams who won't say what they use

Matteo Dapporto
M
Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)Forum Guru (67 reputation)
Group: Forum Members
Posts: 10, Visits: 77
f1rob - 10/11/2018 4:58:36 PM
Matteo Dapporto - 10/11/2018 2:16:52 PM
f1rob - 10/11/2018 2:09:44 PM
Use marbocote 2002
Print your mould
Rub the lines out
Apply 6-10 coats of 2002 depending on the porosity of the part (Can oven between coats)
We nib an smooth with 1200 paper
Apply one last very wet coat an let dry naturally
You will have a mirror like Finnish ( thou you can still polish more) that will be good for anything up to 125deg pre preg
For ultimate shine ( and at a lower temp) use a wax release like freewax from freecote

Thanks!
Does 2002 stick to ABS and PLA materials?
Because in the tech spec it's not mentioned.

MAtteo

Well so far it's worked on every single bit we have done but we make parts for lots of different teams who won't say what they use

So if I well understood the moulds that you are sealing with HP2002 sealer are made by "plastic material"....

f1rob
f1rob
Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)
Group: Forum Members
Posts: 237, Visits: 4.8K
Matteo Dapporto - 10/11/2018 6:56:11 PM
f1rob - 10/11/2018 4:58:36 PM
Matteo Dapporto - 10/11/2018 2:16:52 PM
f1rob - 10/11/2018 2:09:44 PM
Use marbocote 2002
Print your mould
Rub the lines out
Apply 6-10 coats of 2002 depending on the porosity of the part (Can oven between coats)
We nib an smooth with 1200 paper
Apply one last very wet coat an let dry naturally
You will have a mirror like Finnish ( thou you can still polish more) that will be good for anything up to 125deg pre preg
For ultimate shine ( and at a lower temp) use a wax release like freewax from freecote

Thanks!
Does 2002 stick to ABS and PLA materials?
Because in the tech spec it's not mentioned.

MAtteo

Well so far it's worked on every single bit we have done but we make parts for lots of different teams who won't say what they use

So if I well understood the moulds that you are sealing with HP2002 sealer are made by "plastic material"....

All parts are 3d printed,what they are printed with is a mystery ! But 2002 has worked with everything so far

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Matteo - 7 Years Ago
scottracing - 7 Years Ago
Matteo - 7 Years Ago
Hanaldo - 7 Years Ago
Matteo - 7 Years Ago
Hanaldo - 7 Years Ago
Matteo - 7 Years Ago
Steve Broad - 7 Years Ago
Matteo - 7 Years Ago
f1rob - 7 Years Ago
Matteo - 7 Years Ago
f1rob - 7 Years Ago
Matteo - 7 Years Ago
f1rob - 7 Years Ago
scottracing - 7 Years Ago
Furrari - 7 Years Ago
Furrari - 7 Years Ago
Matteo - 7 Years Ago
SleepingAwake - 7 Years Ago
Matteo - 7 Years Ago
SleepingAwake - 7 Years Ago
                     Thanks for your help!
Matteo - 7 Years Ago
Furrari - 7 Years Ago
             End component of the diffuser.
Furrari - 7 Years Ago
scottracing - 7 Years Ago
Furrari - 7 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search