Hello Everyone,

Basically, I've had a go at running before I can walk and stumbled into a problem or 2 I'm hoping somebody can help me with.

The first mould I've had a go at making is for a roll top bath which wasn't going too bad until I had to use Reface to fix any high and low points.
I had never used a spray gun before and didn't do any practice pieces beforehand, I just made sure the gun sprayed properly and jumped in and went for it.

The gun worked okay briefly and then I started having problems with intermittent spraying and no matter what I done, I couldn't get it working properly.
After trying various things the gun seized and was ruined. My fix for this was to brush it on and in my naivety I didn't think it would be too bad... :/

I've gone upto a 40 grit paper and leveled out the brush marks/high points pretty well but, now I have low points where wood is showing through (only a couple of places and nothing too major) and high points where it's still pretty thick Reface (in the corners and where the base meets the walls of the tub) and obviously the scratches from the 40 grit paper..

What I'd like help with is, how is it best to save my hard work, does anybody have any pointers/do's/don'ts before I destroy things further? Should I sand things down and use a paint roller to put on another coat of Reface and start again to a certain extent?

I was thinking to carry on sanding down with finer grit paper, go over any bare bits with more reface (and there maybe a couple of bits that could do with a thin layer of filler first?), and blend it all in with some fine grit paper..

What does anybody think? Any help/ideas are greatly appreciated.. And yes, I know I've been a bit of an impatient arse about all this and I will organise a spray painting course as soon as money permits!

Thanks for your're time reading this, I hope you can help. Rob

Replies
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
If you're in Australia, get in touch with CG Composites and order Scott Bader Primecoat and Glosscoat. Very similar product to what Easy Composites sell.

You really don't want anything that is hard to sand. The more effort you have to put into sanding, the more likely you are digging a hole and won't achieve a flat surface. 

It is generally much harder to spot fill than it is to fill a larger area, because by the time you have got the filled area flat you have dug a low spot around the outside of it. I do a lot of body repair work, and it took me awhile to learn that it is actually much quicker to cover the whole thing and sand it down than it is to try to do small areas because you tend to chase yourself in circles when you do patches.

You are likely going to need to do more than the next coat though, so what you might do is spot fill the low areas, and flat it down with 80 grit (on a block!). Then do another full coat over the entire thing, and with any luck you will get it flat with just that application. If you start to go through again, stop sanding and apply another coat. 
robenergy
robenergy
Supreme Being (185 reputation)Supreme Being (185 reputation)Supreme Being (185 reputation)Supreme Being (185 reputation)Supreme Being (185 reputation)Supreme Being (185 reputation)Supreme Being (185 reputation)Supreme Being (185 reputation)Supreme Being (185 reputation)
Group: Forum Members
Posts: 20, Visits: 216
Hanaldo - 1/9/2018 1:30:56 AM
If you're in Australia, get in touch with CG Composites and order Scott Bader Primecoat and Glosscoat. Very similar product to what Easy Composites sell.

You really don't want anything that is hard to sand. The more effort you have to put into sanding, the more likely you are digging a hole and won't achieve a flat surface. 

It is generally much harder to spot fill than it is to fill a larger area, because by the time you have got the filled area flat you have dug a low spot around the outside of it. I do a lot of body repair work, and it took me awhile to learn that it is actually much quicker to cover the whole thing and sand it down than it is to try to do small areas because you tend to chase yourself in circles when you do patches.

You are likely going to need to do more than the next coat though, so what you might do is spot fill the low areas, and flat it down with 80 grit (on a block!). Then do another full coat over the entire thing, and with any luck you will get it flat with just that application. If you start to go through again, stop sanding and apply another coat. 

I completely get what you're saying about patch filling and creating more work for myself in the long run. The end result is what counts and you gotta put the effort in with the mould!
 
Shame I didn't find CG Composites when I was looking for suppliers! Cheers for the heads up..

I've not spoken to anybody at CG Composites but on the website it says their Bader Primecoat is made for spray guns, where as easy composites is able to be brushed on which suits me just fine at the minute. But I'll ring up first and make sure.

Thanks for the pointers  Hanaldo, muchly appreciated.

PS, one other thing, how finer grit would I have to go down to before I can put my gelcoat on??

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
robenergy - 7 Years Ago
Warren (Staff) - 7 Years Ago
robenergy - 7 Years Ago
Warren (Staff) - 7 Years Ago
robenergy - 7 Years Ago
Hanaldo - 7 Years Ago
robenergy - 7 Years Ago
Hanaldo - 7 Years Ago
robenergy - 7 Years Ago
Hanaldo - 7 Years Ago
robenergy - 7 Years Ago