Hello there,
I've just completed my first infused part. It's a shell for a home made metal detector coil. I'm generally happy with the result but would like to improve the surface finish on future parts.
The part is made with 2 layers of 200gsm fibreglass and a low viscosity epoxy that uses a very slow hardener. It took over 4 hours to start to gel in a warm environment. I'm using a pump that can get down to about -28" and  after I infused the resin it was turned off. No evidence of leaks where seen and the vacuum gauge needle didn't move for the entire cure duration.
If you look at the attached photo of the shell on the scales there are a few areas that appear to have porosity. Small holes between the fibre weave. Could that be caused by using hardener that is too slow and all the resin has been squeezed, drawn out of the very thin laminate? Or is it just evidence of tiny air leaks I couldn't see or measure?
Thanks
Attachments
IMG_2461.JPG (587 views, 1.00 MB)
IMG_2463.JPG (491 views, 2.00 MB)
Reply
oekmont
oekmont
Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)
Group: Forum Members
Posts: 550, Visits: 27K
The mentioned effect has nothing to do with the oxygen bound in the water molecules. Although water molecueles break up from time to time this creates (small amounts of) oh- and h3o+ ions, and no oxygen.
I am talking about physical solution. Every fluid/solid solutes molecules of the surrounding atmosphere. This depends on the substances involved, and the partial pressures. If you reduce the pressure of the system, you reduce the partial pressure of the surrounding atmosphere. As a result the substances in solution leave the liquid.
In our infusion setup, we are talking mostly about water molecules (as far as I know), which solute quite well in epoxy resin.
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Roo2 - 8 Years Ago
oekmont - 8 Years Ago
Roo2 - 8 Years Ago
Warren (Staff) - 8 Years Ago
oekmont - 8 Years Ago
Hanaldo - 8 Years Ago
oekmont - 8 Years Ago
polaraligned - 8 Years Ago
Roo2 - 8 Years Ago
MarkMK - 8 Years Ago
oekmont - 8 Years Ago
Hanaldo - 8 Years Ago
Roo2 - 8 Years Ago
oekmont - 8 Years Ago
Roo2 - 8 Years Ago
Warren (Staff) - 8 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search