Could need some advice on flow front


Author
Message
gnidnu
gnidnu
Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)
Group: Forum Members
Posts: 2, Visits: 193
I'm having trouble with this partly double sided infusion. This was the most recent try. Layup:

(Mould Side)
200 g/m² Glass Twill Weave
300 g/m² Carbon Biaxial +-45°
300 g/m² Glass Biaxial +-45°
400 g/m² Glass Unidirectional 0°
10 mm Gurit Corecell M80 Foam, Perforation Grid 2mm / 20 mm
300 g/m² Glass Biaxial +-45°
200 g/m² Carbon Unidirectional 0°
200 g/m² Carbon Unidirectional 0°
300 g/m² Carbon Biaxial +-45°
160 g/m² Carbon Twill Weave
78 g/m² Glass Twill Weave

MTI hose on left side, feed line on the right.
Can't measure absolute pressure, but relative pressure was -0,93 Bar.
Resin was degassed until no more bubbles were visible.
Didn't turn out well. It looks like the flow front on the A side was significantly slower than on top, which resulted in complete dry spots.

http://www.talkcomposites.com/Uploads/Images/71c93ae2-d2e5-4ad0-b79e-2825.jpg


http://www.talkcomposites.com/Uploads/Images/ef930957-4f0d-49e8-8b4a-4956.jpg

http://www.talkcomposites.com/Uploads/Images/00004841-3815-497c-be93-ac92.jpg

Do you have any advice on what to do differently next time? I already tried infusing from back to front instead of left to right, which turned out better.
Attachments
IMG_20150104_170946-1.jpg (885 views, 177.00 KB)
Edited 11 Years Ago by gnidnu
Reply
ajb100
ajb100
Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)
Group: Forum Members
Posts: 346, Visits: 4.4K
As above, that's a large stack to be working with, slow the resin right down and give it a chance to soak through. Resin doesn't flow vertically through ud/borax as well as woven fabrics so that won't be helping