I'm having trouble with this partly double sided infusion. This was the most recent try. Layup:

(Mould Side)
200 g/m² Glass Twill Weave
300 g/m² Carbon Biaxial +-45°
300 g/m² Glass Biaxial +-45°
400 g/m² Glass Unidirectional 0°
10 mm Gurit Corecell M80 Foam, Perforation Grid 2mm / 20 mm
300 g/m² Glass Biaxial +-45°
200 g/m² Carbon Unidirectional 0°
200 g/m² Carbon Unidirectional 0°
300 g/m² Carbon Biaxial +-45°
160 g/m² Carbon Twill Weave
78 g/m² Glass Twill Weave

MTI hose on left side, feed line on the right.
Can't measure absolute pressure, but relative pressure was -0,93 Bar.
Resin was degassed until no more bubbles were visible.
Didn't turn out well. It looks like the flow front on the A side was significantly slower than on top, which resulted in complete dry spots.

http://www.talkcomposites.com/Uploads/Images/71c93ae2-d2e5-4ad0-b79e-2825.jpg


http://www.talkcomposites.com/Uploads/Images/ef930957-4f0d-49e8-8b4a-4956.jpg

http://www.talkcomposites.com/Uploads/Images/00004841-3815-497c-be93-ac92.jpg

Do you have any advice on what to do differently next time? I already tried infusing from back to front instead of left to right, which turned out better.
Attachments
IMG_20150104_170946-1.jpg (794 views, 177.00 KB)
Edited 11 Years Ago by gnidnu
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search