			            Resin viscosity in my experience is the number one problem. The moment I heated my molds and the resin a lot of the pin hole problems went away.
  My resin viscosity is 300cps. Its thick when cool but at 80F its like water. You want to heat your mold as well so the viscosity of the resin during infusion does not thicken as it would if the mold were too cool.